| Physical Properties | Metric | English | Comments |
|
| Density | 1.33 g/cc | 0.048 lb/in³ | ASTM D 792 |
| Water Absorption | 0.14 % | 0.14 % | 24 hours @ 73F; ASTM D 570 |
| Water Absorption at Saturation | 0.6 % | 0.6 % | Equilibrium, 73F; ASTM D 570 |
| Linear Mold Shrinkage | 0.008 - 0.011 cm/cm | 0.008 - 0.011 in/in | Flow, 30-90 mil; ASTM D 955 |
| Linear Mold Shrinkage | 0.01 - 0.014 cm/cm | 0.01 - 0.014 in/in | Flow, 90-180 mil; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.009 - 0.013 cm/cm | 0.009 - 0.013 in/in | 30-90 mil; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.012 - 0.016 cm/cm | 0.012 - 0.016 in/in | 90-180 mil; ASTM D 955 |
Mechanical Properties |
|
| Hardness, Rockwell R | 115 | 115 | ASTM D 785 |
| Tensile Strength @ Break | 41.4 MPa | 6000 psi | Type I, 2.0 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 41.4 MPa | 6000 psi | Type I, 2.0 in/min; ASTM D 638 |
| Elongation at Break | 120 % | 120 % | Type I, 2.0 in/min; ASTM D 638 |
| Flexural Modulus | 2.24 GPa | 325 ksi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Strength | 68.9 MPa | 10000 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Yield Strength | 68.9 MPa | 10000 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Izod Impact, Notched, Low Temp | 1.71 J/cm | 3.2 ft-lb/in | at -40F; ASTM D 256 |
| Izod Impact, Notched, Low Temp | 1.92 J/cm | 3.6 ft-lb/in | at -22F; ASTM D 256 |
| Gardner Impact | 38 J | 28 ft-lb | 73F; ASTM D 3029 |
| Gardner Impact | 38 J | 28 ft-lb | Modified Gardner, 73F; ASTM D 3029 |
| Izod Impact, Notched | 6.41 J/cm | 12 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Dielectric Constant | 5.7 | 5.7 | 1 MHz; ASTM D 150 |
| Dielectric Constant | 8.5 | 8.5 | 100 Hz; ASTM D 150 |
| Dielectric Strength | 12.1 kV/mm | 307 V/mil | in oil, 125 mils; ASTM D 149 |
| Dissipation Factor | 0.002 | 0.002 | 100 Hz; ASTM D 150 |
| Dissipation Factor | 0.03 | 0.03 | 1 MHz; ASTM D 150 |
| Arc Resistance | 60 - 120 sec | 60 - 120 sec | Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495 |
| Comparative Tracking Index | 175 - 250 V | 175 - 250 V | (+/- 0.125 inch); PLC Code 3; UL 746A |
| Hot Wire Ignition, HWI | 30 - 60 sec | 30 - 60 sec | (+/- 0.125 inch); PLC Code 2; UL 746A |
| High Amp Arc Ignition, HAI | 15 - 30 arcs | 15 - 30 arcs | Surface (+/- 0.125 inch); PLC Code 3; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | 80 - 150 mm/min | 3.15 - 5.91 in/min | (+/- 0.125 inch); PLC Code 3; UL 746A |
Thermal Properties |
|
| CTE, linear 68°F | 68.4 µm/m-°C | 38 µin/in-°F | Flow, -40F to 100F; ASTM E 831 |
| CTE, linear 68°F | 79.2 µm/m-°C | 44 µin/in-°F | Flow, -40F to 200F; ASTM E 831 |
| CTE, linear, 212°F (100°C) | 82.8 µm/m-°C | 46 µin/in-°F | Flow, 140F to 280F; ASTM E 831 |
| Deflection Temperature at 0.46 MPa (66 psi) | 129 °C | 265 °F | 0.250 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 121 °C | 250 °F | 0.250 inch, unannealed; ASTM D 648 |
| UL RTI, Electrical | 105 °C | 221 °F | UL 746B |
| UL RTI, Mechanical with Impact | 105 °C | 221 °F | UL 746B |
| UL RTI, Mechanical without Impact | 105 °C | 221 °F | UL 746B |
| Flammability, UL94 | V-0 | V-0 | 0.03 in. |
| Flammability, UL94 | 7 | 7 | 0.087 in. |
| Oxygen Index | 28.8 % | 28.8 % | ASTM D 2863 |
Descriptive Properties |
|
| CSA File No. | LS88480 | |
| UL File Number, USA | E121562 | |
| UV-light, water exposure/immersion | F2 | UL746C |