Physical PropertiesMetricEnglishComments
Density1.53 g/cc0.0553 lb/in³ ASTM D 792
Water Absorption0.06 %0.06 % 24 hours @ 73F; ASTM D 570
Linear Mold Shrinkage0.003 - 0.005 cm/cm0.003 - 0.005 in/in Flow, 60-125 mil; ASTM D 955
Linear Mold Shrinkage0.005 - 0.008 cm/cm0.005 - 0.008 in/in Flow, 125-180 mil; ASTM D 955
Linear Mold Shrinkage, Transverse0.004 - 0.006 cm/cm0.004 - 0.006 in/in 60-125 mil; ASTM D 955
Linear Mold Shrinkage, Transverse0.006 - 0.009 cm/cm0.006 - 0.009 in/in 125-180 mil; ASTM D 955

Mechanical Properties
Hardness, Rockwell R118118 ASTM D 785
Tensile Strength @ Break119 MPa17300 psi Type I, 0.2 in/min; ASTM D 638
Flexural Modulus7.58 GPa1100 ksi 0.05 in/min, 2" span; ASTM D 790
Flexural Strength190 MPa27500 psi 0.05 in/min, 2" span; ASTM D 790
Izod Impact, Unnotched8.01 J/cm15 ft-lb/in 73F; ASTM D 4812
Izod Impact, Notched0.854 J/cm1.6 ft-lb/in 73F; ASTM D 256

Electrical Properties
Volume ResistivityMin 3.2e+016 ohm-cmMin 3.2e+016 ohm-cm ASTM D 257
Dielectric Constant3.73.7 1 MHz; ASTM D 150
Dielectric Constant3.83.8 100 Hz; ASTM D 150
Dielectric Strength18.7 kV/mm475 V/mil in air, 125 mils; ASTM D 149
Dielectric Strength24.8 kV/mm630 V/mil in oil, 62 mils; ASTM D 149
Dissipation Factor0.0020.002 100 Hz; ASTM D 150
Dissipation Factor0.020.02 1 MHz; ASTM D 150
Arc Resistance120 - 180 sec120 - 180 sec Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495
Comparative Tracking IndexMin 600 VMin 600 V (+/- 0.125 inch); PLC Code 0; UL 746A
High Voltage Arc-Tracking Rate, HVTR10 - 25.4 mm/min0.394 - 1 in/min (+/- 0.125 inch); PLC Code 1; UL 746A

Thermal Properties
CTE, linear 68°F25.2 µm/m-°C14 µin/in-°F Flow, -40F to 100F; ASTM E 831
CTE, linear, 212°F (100°C)25.2 µm/m-°C14 µin/in-°F Flow, 140F to 280F; ASTM E 831
Deflection Temperature at 0.46 MPa (66 psi)216 °C420 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)207 °C405 °F 0.250 inch, unannealed; ASTM D 648
UL RTI, Electrical140 °C284 °F UL 746B
UL RTI, Mechanical with Impact140 °C284 °F UL 746B
UL RTI, Mechanical without Impact140 °C284 °F UL 746B
Flammability, UL94HBHB 0.033 in.
Oxygen Index19 %19 % ASTM D 2863

Descriptive Properties
CSA File No.LS88480 
UL File Number, USAE121562 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.