SABIC Innovative Plastics VALOX 4521 PBT (North America)
Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.53 g/cc | 0.0553 lb/in³ | ASTM D 792 |
Mechanical Properties |
|
| Tensile Strength @ Break | 91 MPa | 13200 psi | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 89.6 MPa | 13000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 2.5 % | 2.5 % | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Yield | 2.4 % | 2.4 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 3.52 GPa | 510 ksi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 4.96 GPa | 720 ksi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Strength | 138 MPa | 20000 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Izod Impact, Unnotched | 4.81 J/cm | 9 ft-lb/in | 73F; ASTM D 4812 |
| Izod Impact, Notched | 0.427 J/cm | 0.8 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Arc Resistance | 120 - 180 sec | 120 - 180 sec | Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495 |
| Comparative Tracking Index | 250 - 400 V | 250 - 400 V | (+/- 0.125 inch); PLC Code 2; UL 746A |
| Hot Wire Ignition, HWI | Min 120 sec | Min 120 sec | (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Amp Arc Ignition, HAI | Min 120 arcs | Min 120 arcs | Surface (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | Min 150 mm/min | Min 5.91 in/min | (+/- 0.125 inch); PLC Code 4; UL 746A |
Thermal Properties |
|
| Deflection Temperature at 0.46 MPa (66 psi) | 219 °C | 426 °F | 0.125 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 205 °C | 401 °F | 0.125 inch, unannealed; ASTM D 648 |
| UL RTI, Electrical | 130 °C | 266 °F | UL 746B |
| UL RTI, Mechanical with Impact | 130 °C | 266 °F | UL 746B |
| UL RTI, Mechanical without Impact | 130 °C | 266 °F | UL 746B |
| Flammability, UL94 | V-0 | V-0 | 0.03 in. |
Descriptive Properties | |
| UL File Number, GLOBAL | E161759 | |
| UL File Number, USA | E121562 | |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |