MatWeb, The Online Materials Database
SABIC Innovative Plastics ULTEM SILTEM-STM1500 Polyetherimide (Europe)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their European product line.
| Physical Properties | Original Value | Comments |
|
| Density | 1.18 g/cc | ASTM D 792 |
| Density | 1.18 g/cc | ISO 1183 |
| Water Absorption at Saturation | 0.12 % | 23C; ISO 62 |
| Linear Mold Shrinkage | 0.012 - 0.014 cm/cm | Flow; ASTM D 955 |
| Melt Flow | 8 g/10 min | cm3/10min; Melt Volume Rate, MVR at 320C/2.16 kg; ISO 1133 |
Mechanical Properties |
|
| Hardness, Shore D | 69 | DIN 53505 |
| Tensile Strength, Ultimate | 25 MPa | 50 mm/min; ISO 527 |
| Tensile Strength, Yield | 20 MPa | 50 mm/min; ISO 527 |
| Elongation at Break | 110 % | 50 mm/min; ISO 527 |
| Elongation at Yield | 15 % | 50 mm/min; ISO 527 |
| Tensile Modulus | 0.59 GPa | 1 mm/min; ISO 527 |
| Flexural Modulus | 0.475 GPa | 2 mm/min; ISO 178 |
| Flexural Strength | 18 MPa | 2 mm/min; ISO 178 |
| Flexural Yield Strength | 20 MPa | 2 mm/min; ISO 178 |
| Izod Impact, Notched (ISO) | 25 kJ/m² | 80*10*4 +23 C; ISO 180/ 1A |
| Izod Impact, Unnotched (ISO) | NB | 80*10*4 +23 C; ISO 180/ 1U |
| Izod Impact, Unnotched Low Temp (ISO) | NB | 80*10*4 -30 C; ISO 180/ 1U |
| Izod Impact, Notched, Low Temp (ISO) | 15 kJ/m² | 80*10*4 -30 C; ISO 180/ 1A |
| Taber Abrasion, mg/1000 Cycles | 60 | CS-17, 1 kg; GE Test |
Electrical Properties |
|
| Volume Resistivity | 4.7e+014 ohm-cm | IEC 60093 |
| Surface Resistivity per Square | Min 1e+015 ohm | ROA; IEC 60093 |
| Dielectric Constant | 3 | 100 Hz; IEC 60250 |
| Dielectric Strength | 19 kV/mm | in oil, 3.2 mm; IEC 60243-1 |
| Dissipation Factor | 0.0091 | 100 Hz; IEC 60250 |
| Comparative Tracking Index | 100 V | M; IEC 60112/3rd |
| Comparative Tracking Index | 175 V | IEC 60112/3rd |
Thermal Properties |
|
| CTE, linear 20°C | 110 µm/m-°C | 23C-80C, flow; ISO 11359-2 |
| CTE, linear 20°C Transverse to Flow | 90 µm/m-°C | 23C-80C; ISO 11359-2 |
| Vicat Softening Point | 75 °C | VST/B/50; DIN 53460 |
| Vicat Softening Point | 75 °C | B/50; ISO 306 |
| Vicat Softening Point | 78 °C | B/120; ISO 306 |
| Flammability, UL94 | V-1 | 1.6 mm; UL 94 by GE |
| Oxygen Index | 48 % | ISO 4589 |
| Glow Wire Test | 960 °C | Passes at 3.2 mm; IEC 60695-2-1 |
Descriptive Properties | |
| Ball Pressure Test, 75 C +/- 2 C | PASSES | IEC 60035-1 |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |