SABIC Innovative Plastics ULTEM 1000 Polyetherimide (Europe)


Subcategory: Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line. This product is also a part of their North American product line.

Physical PropertiesOriginal ValueComments
Density1.27 g/cc ASTM D 792
Density1.27 g/cc ISO 1183
Water Absorption0.25 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.7 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation1.25 % 23C; ISO 62
Linear Mold Shrinkage0.005 - 0.007 cm/cm Flow; ASTM D 955
Melt Flow13 g/10 min cm3/10min; Melt Volume Rate, MVR at 360C/5.0 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell M109 ISO 2039/2
Hardness, H358/30140 MPa ISO 2039/1
Tensile Strength, Ultimate85 MPa 50 mm/min; ISO 527
Tensile Strength, Ultimate90 MPa ASTM D 638
Tensile Strength, Yield105 MPa ASTM D 638
Tensile Strength, Yield105 MPa 50 mm/min; ISO 527
Elongation at Break60 % ASTM D 638
Elongation at Break60 % 50 mm/min; ISO 527
Elongation at Yield6 % 50 mm/min; ISO 527
Elongation at Yield8 % ASTM D 638
Tensile Modulus3 GPa DIN 53457
Tensile Modulus3.2 GPa 1 mm/min; ISO 527
Flexural Modulus3.3 GPa DIN 53457
Flexural Modulus3.3 GPa 2 mm/min; ISO 178
Flexural Yield Strength145 MPa DIN 53452
Flexural Yield Strength160 MPa 2 mm/min; ISO 178
Ultimate Compressive Strength140 MPa ASTM D 695
Compressive Modulus2.9 GPa DIN 53454
Poisson's Ratio0.42 ASTM D 638
Shear Strength100 MPa ASTM D 732
Izod Impact, Notched0.5 J/cm 23 C; ASTM D 256
Izod Impact, Notched (ISO)6 kJ/m² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched13 J/cm 23 C; ASTM D 4812
Izod Impact, Unnotched (ISO)NB 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)NB 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp (ISO)6 kJ/m² 80*10*4 -30 C; ISO 180/ 1A
Charpy Impact, Notched, Low Temp0.4 J/cm² at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Notched0.4 J/cm² 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Notched1 J/cm² 23 C; ISO 179/2C
Gardner Impact36 J GE Test
Taber Abrasion, mg/1000 Cycles10 CS-17, 1 kg; GE Test

Electrical Properties
Volume Resistivity1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant2.9 50 Hz; IEC 60250
Dielectric Constant2.9 1 MHz; IEC 60250
Dielectric Strength16 kV/mm in oil, 3.2 mm; IEC 60243-1
Dielectric Strength25 kV/mm in oil, 1.6 mm; IEC 60243-1
Dielectric Strength33 kV/mm in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.0005 50 Hz; IEC 60250
Dissipation Factor0.0025 2450 MHz; IEC 60250
Dissipation Factor0.006 1 MHz; IEC 60250
Arc Resistance128 sec Tungsten; ASTM D 495
Comparative Tracking Index100 V M; IEC 60112/3rd
Comparative Tracking Index150 V IEC 60112/3rd
Comparative Tracking Index150 V Electr Grey; IEC 60112/3rd

Thermal Properties
CTE, linear 100°C50 µm/m-°C 23C-150C, flow; ISO 11359-2
CTE, linear 100°C50 µm/m-°C 23C-150C, cross flow; ISO 11359-2
Thermal Conductivity0.24 W/m-K ISO 8302
Deflection Temperature at 0.46 MPa (66 psi)200 °C HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 0.46 MPa (66 psi)210 °C ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)190 °C HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Deflection Temperature at 1.8 MPa (264 psi)200 °C ASTM D 648
Vicat Softening Point211 °C B/50; ISO 306
Vicat Softening Point212 °C B/120; ISO 306
Vicat Softening Point215 °C A/50; ISO 306
Vicat Softening Point219 °C Rate B; ASTM D 1525
Vicat Softening Point219 °C VST/A/120; DIN 53460
UL RTI, Electrical170 °C UL 746B
UL RTI, Mechanical with Impact170 °C UL 746B
UL RTI, Mechanical without Impact170 °C UL 746B
Flammability, UL94V-0 0.41 mm
Flammability, UL947 94-1.9 mm
Flammability Test1 mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2
NBS Smoke Density0.7 Flaming, Ds 4 min; ASTM E 662
NBS Smoke Density30 Flaming, Dmax 20 min; ASTM E 662
Oxygen Index47 % ISO 4589
Glow Wire Test960 °C Passes at 3.2 mm; EDF HN60S02
Glow Wire Test960 °C Passes at 3.2 mm; IEC 60695-2-1

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1
Hot Mandrel Test, 300 CPASSES CEE10/IIed
MPa; Hardness, H961/30200 DIN 53456
Needle Flame Test, 3.2 mm, Burn Time sPASSES IEC 60695-2-2

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.