Physical PropertiesMetricEnglishComments
Density1.27 g/cc0.0459 lb/in³ ASTM D 792
Density1.27 g/cc0.0459 lb/in³ ISO 1183
Water Absorption0.25 %0.25 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.7 %0.7 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation1.25 %1.25 % 23C; ISO 62
Linear Mold Shrinkage0.005 - 0.007 cm/cm0.005 - 0.007 in/in Flow; ASTM D 955
Melt Flow13 g/10 min13 g/10 min cm3/10min; Melt Volume Rate, MVR at 360C/5.0 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell M109109 ISO 2039/2
Hardness, H358/30140 MPa20300 psi ISO 2039/1
Tensile Strength, Ultimate85 MPa12300 psi 50 mm/min; ISO 527
Tensile Strength, Ultimate90 MPa13100 psi ASTM D 638
Tensile Strength, Yield105 MPa15200 psi ASTM D 638
Tensile Strength, Yield105 MPa15200 psi 50 mm/min; ISO 527
Elongation at Break60 %60 % ASTM D 638
Elongation at Break60 %60 % 50 mm/min; ISO 527
Elongation at Yield6 %6 % 50 mm/min; ISO 527
Elongation at Yield8 %8 % ASTM D 638
Tensile Modulus3 GPa435 ksi DIN 53457
Tensile Modulus3.2 GPa464 ksi 1 mm/min; ISO 527
Flexural Modulus3.3 GPa479 ksi DIN 53457
Flexural Modulus3.3 GPa479 ksi 2 mm/min; ISO 178
Flexural Yield Strength145 MPa21000 psi DIN 53452
Flexural Yield Strength160 MPa23200 psi 2 mm/min; ISO 178
Ultimate Compressive Strength140 MPa20300 psi ASTM D 695
Compressive Modulus2.9 GPa421 ksi DIN 53454
Shear Strength100 MPa14500 psi ASTM D 732
Izod Impact, Notched0.5 J/cm0.937 ft-lb/in 23 C; ASTM D 256
Izod Impact, Notched (ISO)6 kJ/m²2.86 ft-lb/in² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched13 J/cm24.4 ft-lb/in 23 C; ASTM D 4812
Izod Impact, Unnotched (ISO)NBNB 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)NBNB 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp (ISO)6 kJ/m²2.86 ft-lb/in² 80*10*4 -30 C; ISO 180/ 1A
Charpy Impact, Notched, Low Temp0.4 J/cm²1.9 ft-lb/in² at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Notched0.4 J/cm²1.9 ft-lb/in² 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Notched1 J/cm²4.76 ft-lb/in² 23 C; ISO 179/2C
Taber Abrasion, mg/1000 Cycles1010 CS-17, 1 kg; GE Test

Electrical Properties
Volume Resistivity1e+015 ohm-cm1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohmMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant2.92.9 50 Hz; IEC 60250
Dielectric Constant2.92.9 1 MHz; IEC 60250
Dielectric Strength16 kV/mm406 kV/in in oil, 3.2 mm; IEC 60243-1
Dielectric Strength25 kV/mm635 kV/in in oil, 1.6 mm; IEC 60243-1
Dielectric Strength33 kV/mm838 kV/in in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.00050.0005 50 Hz; IEC 60250
Dissipation Factor0.00250.0025 2450 MHz; IEC 60250
Dissipation Factor0.0060.006 1 MHz; IEC 60250
Arc Resistance128 sec128 sec Tungsten; ASTM D 495
Comparative Tracking Index100 V100 V M; IEC 60112/3rd
Comparative Tracking Index150 V150 V IEC 60112/3rd

Thermal Properties
CTE, linear 100°C50 µm/m-°C27.8 µin/in-°F 23C-150C, flow; ISO 11359-2
CTE, linear 100°C50 µm/m-°C27.8 µin/in-°F 23C-150C, cross flow; ISO 11359-2
Thermal Conductivity0.24 W/m-K1.67 BTU-in/hr-ft²-°F ISO 8302
Deflection Temperature at 0.46 MPa (66 psi)200 °C392 °F HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 0.46 MPa (66 psi)210 °C410 °F ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)190 °C374 °F HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Deflection Temperature at 1.8 MPa (264 psi)200 °C392 °F ASTM D 648
Vicat Softening Point211 °C412 °F B/50; ISO 306
Vicat Softening Point215 °C419 °F A/50; ISO 306
Vicat Softening Point215 °C419 °F B/120; ISO 306
Vicat Softening Point219 °C426 °F Rate B; ASTM D 1525
UL RTI, Electrical170 °C338 °F UL 746B
UL RTI, Mechanical with Impact170 °C338 °F UL 746B
UL RTI, Mechanical without Impact170 °C338 °F UL 746B
Flammability, UL94V-0V-0 0.41 mm
Flammability, UL9477 94-1.9 mm
NBS Smoke Density0.70.7 Flaming, Ds 4 min; ASTM E 662
NBS Smoke Density3030 Flaming, Dmax 20 min; ASTM E 662
Oxygen Index47 %47 % ISO 4589
Glow Wire Test960 °C1760 °F Passes at 3.2 mm; IEC 60695-2-1

Descriptive Properties
MPa; Hardness, H961/30200 DIN 53456

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.