SABIC Innovative Plastics ULTEM 2200 Polyetherimide (Europe)


Subcategory: Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line. This product is also a part of their North American product line.

Physical PropertiesMetricEnglishComments
Density1.42 g/cc0.0513 lb/in³ ASTM D 792
Density1.42 g/cc0.0513 lb/in³ ISO 1183
Filler Content20 %20 % ASTM D 229
Water Absorption0.26 %0.26 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.55 %0.55 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation1 %1 % 23C; ISO 62
Linear Mold Shrinkage0.003 - 0.005 cm/cm0.003 - 0.005 in/in Flow; ASTM D 955
Melt Flow7 g/10 min7 g/10 min cm3/10min; Melt Volume Rate, MVR at 360C/5.0 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell M114114 ISO 2039/2
Hardness, H358/30150 MPa21800 psi ISO 2039/1
Tensile Strength, Ultimate140 MPa20300 psi 5 mm/min; ISO 527
Tensile Strength, Ultimate140 MPa20300 psi ASTM D 638
Elongation at Break2 %2 % 5 mm/min; ISO 527
Elongation at Break3 %3 % ASTM D 638
Tensile Modulus6.8 GPa986 ksi 1 mm/min; ISO 527
Tensile Modulus6.9 GPa1000 ksi DIN 53457
Flexural Modulus6.5 GPa943 ksi 2 mm/min; ISO 178
Flexural Modulus6.8 GPa986 ksi DIN 53457
Flexural Strength200 MPa29000 psi DIN 53452
Flexural Strength210 MPa30500 psi 2 mm/min; ISO 178
Ultimate Compressive Strength170 MPa24700 psi ASTM D 695
Compressive Modulus6 GPa870 ksi DIN 53454
Poisson's Ratio0.380.38 ASTM D 638
Shear Strength95 MPa13800 psi ASTM D 732
Izod Impact, Notched0.9 J/cm1.69 ft-lb/in 23 C; ASTM D 256
Izod Impact, Unnotched4.8 J/cm8.99 ft-lb/in 23 C; ASTM D 4812
Izod Impact, Unnotched (ISO)30 kJ/m²14.3 ft-lb/in² 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)30 kJ/m²14.3 ft-lb/in² 80*10*4 -30 C; ISO 180/ 1U
Charpy Impact Unnotched3.5 J/cm²16.7 ft-lb/in² 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Unnotched Low Temp3.5 J/cm²16.7 ft-lb/in² at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched0.9 J/cm²4.28 ft-lb/in² 23 C; ISO 179/2C
Taber Abrasion, mg/1000 Cycles1717 CS-17, 1 kg; GE Test

Electrical Properties
Volume Resistivity1e+015 ohm-cm1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohmMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant33 1 MHz; IEC 60250
Dielectric Constant3.13.1 60 Hz; IEC 60250
Dielectric Constant3.13.1 50 Hz; IEC 60250
Dielectric Strength16 kV/mm406 kV/in in oil, 3.2 mm; IEC 60243-1
Dielectric Strength26 kV/mm660 kV/in in oil, 1.6 mm; IEC 60243-1
Dielectric Strength34 kV/mm864 kV/in in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.00080.0008 50 Hz; IEC 60250
Dissipation Factor0.00250.0025 1 MHz; IEC 60250
Dissipation Factor0.00490.0049 2450 MHz; IEC 60250
Arc Resistance85 sec85 sec Tungsten; ASTM D 495
Comparative Tracking Index100 V100 V M; IEC 60112/3rd
Comparative Tracking Index150 V150 V IEC 60112/3rd
Comparative Tracking Index150 V150 V Stand. Black; IEC 60112/3rd

Thermal Properties
CTE, linear 100°C25 µm/m-°C13.9 µin/in-°F 23C-150C, flow; ISO 11359-2
CTE, linear 100°C60 µm/m-°C33.3 µin/in-°F 23C-150C, cross flow; ISO 11359-2
Thermal Conductivity0.28 W/m-K1.94 BTU-in/hr-ft²-°F ISO 8302
Deflection Temperature at 0.46 MPa (66 psi)210 °C410 °F ASTM D 648
Deflection Temperature at 0.46 MPa (66 psi)210 °C410 °F HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi)205 °C401 °F HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Deflection Temperature at 1.8 MPa (264 psi)209 °C408 °F ASTM D 648
Vicat Softening Point212 °C414 °F B/50; ISO 306
Vicat Softening Point218 °C424 °F B/120; ISO 306
Vicat Softening Point223 °C433 °F A/50; ISO 306
Vicat Softening Point226 °C439 °F Rate B; ASTM D 1525
Vicat Softening Point226 °C439 °F VST/A/120; DIN 53460
UL RTI, Electrical170 °C338 °F UL 746B
UL RTI, Mechanical with Impact170 °C338 °F UL 746B
UL RTI, Mechanical without Impact170 °C338 °F UL 746B
Flammability, UL94V-0V-0 0.41 mm
Flammability, UL9477 94-1.9 mm
Flammability Test11 mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2
NBS Smoke Density1.31.3 Flaming, Ds 4 min; ASTM E 662
NBS Smoke Density2727 Flaming, Dmax 20 min; ASTM E 662
Oxygen Index46 %46 % ISO 4589
Glow Wire Test960 °C1760 °F Passes at 3.2 mm; IEC 60695-2-1
Glow Wire Test960 °C1760 °F Passes at 3.2 mm; EDF HN60S02

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1
Hot Mandrel Test, 300 CPASSES CEE10/IIed
MPa; Hardness, H961/30265 DIN 53456
Needle Flame Test, 3.2 mm, Burn Time sPASSES IEC 60695-2-2

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.