Physical PropertiesOriginal ValueComments
Density1.51 g/cc ASTM D 792
Density1.51 g/cc ISO 1183
Filler Content30 % ASTM D 229
Water Absorption0.18 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.5 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.9 % 23C; ISO 62
Linear Mold Shrinkage0.002 - 0.004 cm/cm Flow; ASTM D 955
Melt Flow6 g/10 min cm3/10min; Melt Volume Rate, MVR at 360C/5.0 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell M114 ISO 2039/2
Hardness, H358/30165 MPa ISO 2039/1
Tensile Strength, Ultimate160 MPa ASTM D 638
Tensile Strength, Ultimate165 MPa 5 mm/min; ISO 527
Elongation at Break2 % 5 mm/min; ISO 527
Elongation at Break3 % ASTM D 638
Tensile Modulus9 GPa DIN 53457
Tensile Modulus9.5 GPa 1 mm/min; ISO 527
Flexural Modulus8.1 GPa DIN 53457
Flexural Modulus8.5 GPa 2 mm/min; ISO 178
Flexural Strength225 MPa 2 mm/min; ISO 178
Flexural Strength230 MPa DIN 53452
Ultimate Compressive Strength175 MPa ASTM D 695
Compressive Modulus7.5 GPa DIN 53454
Poisson's Ratio0.38 ASTM D 638
Shear Strength100 MPa ASTM D 732
Izod Impact, Notched1 J/cm 23 C; ASTM D 256
Izod Impact, Unnotched4.3 J/cm 23 C; ASTM D 4812
Izod Impact, Unnotched (ISO)40 kJ/m² 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)40 kJ/m² 80*10*4 -30 C; ISO 180/ 1U
Charpy Impact Unnotched4 J/cm² 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Unnotched Low Temp4 J/cm² at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched1 J/cm² 23 C; ISO 179/2C
Taber Abrasion, mg/1000 Cycles20 CS-17, 1 kg; GE Test

Electrical Properties
Volume Resistivity1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant3.3 50 Hz; IEC 60250
Dielectric Constant3.4 1 MHz; IEC 60250
Dielectric Strength15 kV/mm in oil, 3.2 mm; IEC 60243-1
Dielectric Strength26 kV/mm in oil, 1.6 mm; IEC 60243-1
Dielectric Strength35 kV/mm in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.0016 50 Hz; IEC 60250
Dissipation Factor0.0023 1 MHz; IEC 60250
Dissipation Factor0.0053 2450 MHz; IEC 60250
Arc Resistance85 sec Tungsten; ASTM D 495
Comparative Tracking Index100 V M; IEC 60112/3rd
Comparative Tracking Index150 V IEC 60112/3rd
Comparative Tracking Index150 V Stand. Black; IEC 60112/3rd

Thermal Properties
CTE, linear 100°C20 µm/m-°C 23C-150C, flow; ISO 11359-2
CTE, linear 100°C60 µm/m-°C 23C-150C, cross flow; ISO 11359-2
Thermal Conductivity0.29 W/m-K ISO 8302
Deflection Temperature at 0.46 MPa (66 psi)212 °C ASTM D 648
Deflection Temperature at 0.46 MPa (66 psi)215 °C HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi)210 °C ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)210 °C HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point213 °C B/50; ISO 306
Vicat Softening Point220 °C B/120; ISO 306
Vicat Softening Point225 °C A/50; ISO 306
Vicat Softening Point228 °C Rate B; ASTM D 1525
Vicat Softening Point228 °C VST/A/120; DIN 53460
UL RTI, Electrical180 °C UL 746B
UL RTI, Mechanical with Impact170 °C UL 746B
UL RTI, Mechanical without Impact180 °C UL 746B
Flammability, UL94V-0 0.25 mm
Flammability, UL947 94-1.2 mm
Flammability Test1 mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2
NBS Smoke Density1.6 Flaming, Ds 4 min; ASTM E 662
NBS Smoke Density20 Flaming, Dmax 20 min; ASTM E 662
Oxygen Index48 % ISO 4589
Glow Wire Test960 °C Passes at 3.2 mm; EDF HN60S02
Glow Wire Test960 °C Passes at 3.2 mm; IEC 60695-2-1

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1
Hot Mandrel Test, 300 CPASSES CEE10/IIed
MPa; Hardness, H961/30290 DIN 53456
Needle Flame Test, 3.2 mm, Burn Time sPASSES IEC 60695-2-2

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.