MatWeb, The Online Materials Database

SABIC Innovative Plastics ULTEM 2400 Polyetherimide (Europe)


Subcategory: Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line. This product is also a part of their North American product line.

Physical PropertiesMetricEnglishComments
Density1.61 g/cc0.0582 lb/in³ ASTM D 792
Density1.61 g/cc0.0582 lb/in³ ISO 1183
Filler Content40 %40 % ASTM D 229
Water Absorption0.12 %0.12 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.4 %0.4 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.8 %0.8 % 23C; ISO 62
Linear Mold Shrinkage0.001 - 0.003 cm/cm0.001 - 0.003 in/in Flow; ASTM D 955
Melt Flow5 g/10 min5 g/10 min cm3/10min; Melt Volume Rate, MVR at 360C/5.0 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell M125125 ISO 2039/2
Hardness, H358/30170 MPa24700 psi ISO 2039/1
Tensile Strength, Ultimate180 MPa26100 psi 5 mm/min; ISO 527
Tensile Strength, Ultimate186 MPa27000 psi ASTM D 638
Elongation at Break2 %2 % 5 mm/min; ISO 527
Elongation at Break2.5 %2.5 % ASTM D 638
Tensile Modulus11.5 GPa1670 ksi 1 mm/min; ISO 527
Tensile Modulus11.7 GPa1700 ksi DIN 53457
Flexural Modulus10 GPa1450 ksi 2 mm/min; ISO 178
Flexural Modulus11.7 GPa1700 ksi DIN 53457
Flexural Strength240 MPa34800 psi 2 mm/min; ISO 178
Flexural Strength250 MPa36300 psi DIN 53452
Ultimate Compressive Strength200 MPa29000 psi ASTM D 695
Compressive Modulus10 GPa1450 ksi DIN 53454
Shear Strength103 MPa14900 psi ASTM D 732
Izod Impact, Notched1.05 J/cm1.97 ft-lb/in 23 C; ASTM D 256
Izod Impact, Unnotched4.3 J/cm8.06 ft-lb/in 23 C; ASTM D 4812
Izod Impact, Unnotched (ISO)35 kJ/m²16.7 ft-lb/in² 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)35 kJ/m²16.7 ft-lb/in² 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp1.05 J/cm1.97 ft-lb/in at -40 C; ASTM D 256
Charpy Impact Unnotched4 J/cm²19 ft-lb/in² 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Unnotched Low Temp4 J/cm²19 ft-lb/in² at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Taber Abrasion, mg/1000 Cycles2020 CS-17, 1 kg; GE Test

Electrical Properties
Volume Resistivity1e+015 ohm-cm1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohmMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant3.13.1 1 MHz; IEC 60250
Dielectric Constant3.53.5 50 Hz; IEC 60250
Dielectric Strength16 kV/mm406 kV/in in oil, 3.2 mm; IEC 60243-1
Dielectric Strength26 kV/mm660 kV/in in oil, 1.6 mm; IEC 60243-1
Dielectric Strength35 kV/mm889 kV/in in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.00190.0019 1 MHz; IEC 60250
Dissipation Factor0.00250.0025 50 Hz; IEC 60250
Arc Resistance85 sec85 sec Tungsten; ASTM D 495
Comparative Tracking Index100 V100 V M; IEC 60112/3rd
Comparative Tracking Index150 V150 V IEC 60112/3rd
Comparative Tracking Index150 V150 V Stand. Black; IEC 60112/3rd

Thermal Properties
CTE, linear 100°C15 µm/m-°C8.33 µin/in-°F 23C-150C, flow; ISO 11359-2
CTE, linear 100°C45 µm/m-°C25 µin/in-°F 23C-150C, cross flow; ISO 11359-2
Thermal Conductivity0.33 W/m-K2.29 BTU-in/hr-ft²-°F ISO 8302
Deflection Temperature at 0.46 MPa (66 psi)215 °C419 °F HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 0.46 MPa (66 psi)216 °C421 °F ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)210 °C410 °F HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Deflection Temperature at 1.8 MPa (264 psi)213 °C415 °F ASTM D 648
Vicat Softening Point217 °C423 °F B/50; ISO 306
Vicat Softening Point225 °C437 °F B/120; ISO 306
Vicat Softening Point230 °C446 °F A/50; ISO 306
Vicat Softening Point234 °C453 °F VST/A/120; DIN 53460
UL RTI, Electrical170 °C338 °F UL 746B
UL RTI, Mechanical with Impact170 °C338 °F UL 746B
UL RTI, Mechanical without Impact170 °C338 °F UL 746B
Flammability, UL94V-0V-0 0.25 mm
Flammability Test11 mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2
NBS Smoke Density11 Flaming, Ds 4 min; ASTM E 662
NBS Smoke Density2020 Flaming, Dmax 20 min; ASTM E 662
Oxygen Index48 %48 % ISO 4589
Glow Wire Test960 °C1760 °F Passes at 3.2 mm; EDF HN60S02
Glow Wire Test960 °C1760 °F Passes at 3.2 mm; IEC 60695-2-1

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.