Physical Properties | Metric | English | Comments |
|
Density | 1.3 g/cc | 0.047 lb/in³ | ISO 1183 |
Density | 1.32 g/cc | 0.0477 lb/in³ | ASTM D 792 |
Moisture Absorption at Equilibrium | 0.7 % | 0.7 % | (23 C / 50% RH) 1L; ISO 15512 |
Water Absorption at Saturation | 1.25 % | 1.25 % | 23C; ISO 62 |
Linear Mold Shrinkage | 0.006 - 0.008 cm/cm | 0.006 - 0.008 in/in | Flow; ASTM D 955 |
Melt Flow | 22 g/10 min | 22 g/10 min | cm3/10min; Melt Volume Rate, MVR at 360C/5.0 kg; ISO 1133 |
Mechanical Properties |
|
Hardness, H358/30 | 145 MPa | 21000 psi | ISO 2039/1 |
Tensile Strength, Ultimate | 70 MPa | 10200 psi | 50 mm/min; ISO 527 |
Tensile Strength, Yield | 95 MPa | 13800 psi | 50 mm/min; ISO 527 |
Elongation at Break | 50 % | 50 % | 50 mm/min; ISO 527 |
Elongation at Yield | 6 % | 6 % | 50 mm/min; ISO 527 |
Tensile Modulus | 3 GPa | 435 ksi | 1 mm/min; ISO 527 |
Flexural Modulus | 3 GPa | 435 ksi | 2 mm/min; ISO 178 |
Flexural Yield Strength | 135 MPa | 19600 psi | 2 mm/min; ISO 178 |
Izod Impact, Notched (ISO) | 6 kJ/m² | 2.86 ft-lb/in² | 80*10*4 +23 C; ISO 180/ 1A |
Izod Impact, Notched, Low Temp (ISO) | 6 kJ/m² | 2.86 ft-lb/in² | 80*10*4 -30 C; ISO 180/ 1A |
Charpy Impact, Notched, Low Temp | 0.6 J/cm² | 2.86 ft-lb/in² | at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Charpy Impact, Notched | 0.6 J/cm² | 2.86 ft-lb/in² | 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Electrical Properties |
|
Volume Resistivity | Min 1e+015 ohm-cm | Min 1e+015 ohm-cm | IEC 60093 |
Surface Resistivity per Square | Min 1e+015 ohm | Min 1e+015 ohm | ROA; IEC 60093 |
Dielectric Constant | 2.8 | 2.8 | 1 MHz; IEC 60250 |
Dielectric Constant | 2.9 | 2.9 | 50 Hz; IEC 60250 |
Dielectric Strength | 18 kV/mm | 457 kV/in | in oil, 3.2 mm; IEC 60243-1 |
Dissipation Factor | 0.005 | 0.005 | 1 MHz; IEC 60250 |
Comparative Tracking Index | 150 V | 150 V | IEC 60112/3rd |
Thermal Properties |
|
CTE, linear 100°C | 55 µm/m-°C | 30.6 µin/in-°F | 23C-150C, flow; ISO 11359-2 |
CTE, linear 100°C | 55 µm/m-°C | 30.6 µin/in-°F | 23C-150C, cross flow; ISO 11359-2 |
Thermal Conductivity | 0.26 W/m-K | 1.8 BTU-in/hr-ft²-°F | ISO 8302 |
Deflection Temperature at 0.46 MPa (66 psi) | 195 °C | 383 °F | HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be |
Deflection Temperature at 1.8 MPa (264 psi) | 175 °C | 347 °F | HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae |
Vicat Softening Point | 200 °C | 392 °F | B/50; ISO 306 |
Vicat Softening Point | 200 °C | 392 °F | B/120; ISO 306 |
Vicat Softening Point | 210 °C | 410 °F | A/50; ISO 306 |
Oxygen Index | 50 % | 50 % | ISO 4589 |
Glow Wire Test | 960 °C | 1760 °F | Passes at 3.2 mm; IEC 60695-2-1 |
Descriptive Properties |
|
Ball Pressure Test, 125 C +/- 2 C | PASSES | IEC 60035-1 |