SABIC Innovative Plastics VALOX DR51 PBT (Europe)


Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line. This product is also a part of their North American product line.

Physical PropertiesMetricEnglishComments
Density1.41 g/cc0.0509 lb/in³ ASTM D 792
Density1.41 g/cc0.0509 lb/in³ ISO 1183
Water Absorption0.07 %0.07 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.07 %0.07 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.2 %0.2 % 23C; ISO 62
Linear Mold Shrinkage0.005 - 0.008 cm/cm0.005 - 0.008 in/in Flow; ASTM D 955
Linear Mold Shrinkage, Transverse0.006 - 0.009 cm/cm0.006 - 0.009 in/in ASTM D 955
Melt Flow15 g/10 min15 g/10 min cm3/10min; Melt Volume Rate, MVR at 250C/2.16 kg; ISO 1133
Melt Flow18 g/10 min18 g/10 min 250C/2.16 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell R118118 ISO 2039/2
Hardness, H358/30115 MPa16700 psi ISO 2039/1
Tensile Strength, Ultimate100 MPa14500 psi 5 mm/min; ISO 527
Elongation at Break3 %3 % 5 mm/min; ISO 527
Tensile Modulus5.6 GPa812 ksi 1 mm/min; ISO 527
Flexural Modulus5.1 GPa740 ksi 2 mm/min; ISO 178
Flexural Strength145 MPa21000 psi DIN 53452
Flexural Strength155 MPa22500 psi 2 mm/min; ISO 178
Izod Impact, Notched0.55 J/cm1.03 ft-lb/in 23 C; ASTM D 256
Izod Impact, Notched (ISO)5 kJ/m²2.38 ft-lb/in² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched (ISO)30 kJ/m²14.3 ft-lb/in² 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)30 kJ/m²14.3 ft-lb/in² 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp (ISO)4 kJ/m²1.9 ft-lb/in² 80*10*4 -30 C; ISO 180/ 1A
Izod Impact, Notched, Low Temp (ISO)5 kJ/m²2.38 ft-lb/in² 80*10*4 -20 C; ISO 180/ 1A
Izod Impact, Notched, Low Temp (ISO)5 kJ/m²2.38 ft-lb/in² 80*10*4 -40 C; ISO 180/ 1A
Charpy Impact Unnotched3 J/cm²14.3 ft-lb/in² 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched, Low Temp0.4 J/cm²1.9 ft-lb/in² at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Unnotched Low Temp3 J/cm²14.3 ft-lb/in² at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched0.5 J/cm²2.38 ft-lb/in² 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Taber Abrasion, mg/1000 Cycles1616 CS-17, 1 kg; GE Test

Electrical Properties
Volume Resistivity1e+015 ohm-cm1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohmMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant2.92.9 1 MHz; IEC 60250
Dielectric Constant33 50 Hz; IEC 60250
Dielectric Strength18 kV/mm457 kV/in in oil, 3.2 mm; IEC 60243-1
Dielectric Strength20 kV/mm508 kV/in Short time, 3.2 mm; ASTM D 149
Dielectric Strength24 kV/mm610 kV/in in oil, 1.6 mm; IEC 60243-1
Dielectric Strength26 kV/mm660 kV/in in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.0010.001 50 Hz; IEC 60250
Dissipation Factor0.0150.015 1 MHz; IEC 60250
Arc Resistance129 sec129 sec Tungsten; ASTM D 495
Comparative Tracking Index250 V250 V Stand. Black; IEC 60112/3rd
Comparative Tracking Index275 V275 V Electr Grey; IEC 60112/3rd
Comparative Tracking Index300 V300 V IEC 60112/3rd
Hot Wire Ignition, HWI16 sec16 sec UL 746A
High Amp Arc Ignition, HAI112 arcs112 arcs on surface; UL 746A
High Voltage Arc-Tracking Rate, HVTR0.9 mm/min0.0354 in/min UL 746A

Thermal Properties
CTE, linear 20°C35 µm/m-°C19.4 µin/in-°F 23C-80C, flow; ISO 11359-2
CTE, linear 20°C Transverse to Flow95 µm/m-°C52.8 µin/in-°F 23C-80C; ISO 11359-2
CTE, linear 100°C100 µm/m-°C55.6 µin/in-°F 23C-150C, cross flow; ISO 11359-2
Thermal Conductivity0.19 W/m-K1.32 BTU-in/hr-ft²-°F ISO 8302
Deflection Temperature at 0.46 MPa (66 psi)210 °C410 °F ASTM D 648
Deflection Temperature at 0.46 MPa (66 psi)210 °C410 °F HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi)175 °C347 °F HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Deflection Temperature at 1.8 MPa (264 psi)190 °C374 °F ASTM D 648
Vicat Softening Point200 °C392 °F B/50; ISO 306
Vicat Softening Point200 °C392 °F B/120; ISO 306
Vicat Softening Point210 °C410 °F Rate B; ASTM D 1525
Vicat Softening Point213 °C415 °F VST/A/120; DIN 53460
UL RTI, Electrical130 °C266 °F UL 746B
UL RTI, Mechanical with Impact130 °C266 °F UL 746B
UL RTI, Mechanical without Impact140 °C284 °F UL 746B
Flammability, UL94HBHB 0.75 mm
Glow Wire Test750 °C1380 °F Passes at 1 mm; EDF HN60S02
Glow Wire Test750 °C1380 °F Passes at 1 mm; IEC 60695-2-1

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.