MatWeb, The Online Materials Database

SABIC Innovative Plastics VALOX 357X PBT (Europe)


Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line.

Physical PropertiesOriginal ValueComments
Density1.34 g/cc ASTM D 792
Density1.34 g/cc ISO 1183
Water Absorption0.08 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.15 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.5 % 23C; ISO 62
Linear Mold Shrinkage0.011 - 0.018 cm/cm Flow; ASTM D 955
Linear Mold Shrinkage, Transverse0.009 - 0.018 cm/cm ASTM D 955
Melt Flow8 g/10 min cm3/10min; Melt Volume Rate, MVR at 250C/5.0 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell R117 ISO 2039/2
Hardness, H358/30111 MPa ISO 2039/1
Tensile Strength, Ultimate40 MPa ASTM D 638
Tensile Strength, Ultimate40 MPa 50 mm/min; ISO 527
Tensile Strength, Yield50 MPa ASTM D 638
Tensile Strength, Yield50 MPa 50 mm/min; ISO 527
Elongation at Break120 % ASTM D 638
Elongation at Break30 % 50 mm/min; ISO 527
Elongation at Yield5 % ASTM D 638
Elongation at Yield5 % 50 mm/min; ISO 527
Tensile Modulus2.1 GPa DIN 53457
Tensile Modulus2.2 GPa 1 mm/min; ISO 527
Flexural Modulus2 GPa DIN 53457
Flexural Modulus2 GPa 2 mm/min; ISO 178
Flexural Yield Strength80 MPa 2 mm/min; ISO 178
Flexural Yield Strength85 MPa DIN 53452
Izod Impact, Notched5 J/cm 23 C; ASTM D 256
Izod Impact, Notched (ISO)45 kJ/m² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched (ISO)NB 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)NB 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp (ISO)10 kJ/m² 80*10*4 -30 C; ISO 180/ 1A
Charpy Impact UnnotchedNB 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched, Low Temp2 J/cm² at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Unnotched Low TempNB at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched1.5 J/cm² 23 C; ISO 179/2C
Charpy Impact, Notched4.5 J/cm² 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Taber Abrasion, mg/1000 Cycles33 CS-17, 1 kg; GE Test

Electrical Properties
Volume ResistivityMin 1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant2.9 1 MHz; IEC 60250
Dielectric Constant3 50 Hz; IEC 60250
Dielectric Strength18 kV/mm in oil, 3.2 mm; IEC 60243-1
Dielectric Strength21 kV/mm Short time, 3.2 mm; ASTM D 149
Dielectric Strength26 kV/mm in oil, 1.6 mm; IEC 60243-1
Dielectric Strength34 kV/mm in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.002 50 Hz; IEC 60250
Dissipation Factor0.007 1 MHz; IEC 60250
Arc Resistance71 sec Tungsten; ASTM D 495
Comparative Tracking Index100 V M; IEC 60112/3rd
Comparative Tracking Index225 V IEC 60112/3rd
Comparative Tracking Index225 V Stand. Black; IEC 60112/3rd
Comparative Tracking Index250 V Electr Grey; IEC 60112/3rd
Hot Wire Ignition, HWI37 sec UL 746A
High Amp Arc Ignition, HAI28 arcs on surface; UL 746A
High Voltage Arc-Tracking Rate, HVTR8.1 mm/min UL 746A

Thermal Properties
CTE, linear 20°C100 µm/m-°C 23C-80C, flow; ISO 11359-2
CTE, linear 20°C Transverse to Flow100 µm/m-°C 23C-80C; ISO 11359-2
Thermal Conductivity0.17 W/m-K ISO 8302
Deflection Temperature at 0.46 MPa (66 psi)135 °C HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 0.46 MPa (66 psi)138 °C ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)100 °C ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)85 °C HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point145 °C B/50; ISO 306
Vicat Softening Point150 °C B/120; ISO 306
Vicat Softening Point180 °C A/50; ISO 306
Vicat Softening Point183 °C Rate B; ASTM D 1525
Vicat Softening Point183 °C VST/A/120; DIN 53460
UL RTI, Electrical120 °C UL 746B
UL RTI, Mechanical with Impact120 °C UL 746B
UL RTI, Mechanical without Impact140 °C UL 746B
Flammability, UL94V-0 0.75 mm
Flammability, UL947 94-2 mm
Flammability Test1.6 mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2
Oxygen Index30 % ISO 4589
Glow Wire Test960 °C Passes at 1 mm; EDF HN60S02
Glow Wire Test960 °C Passes at 1 mm; IEC 60695-2-1

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1
Hot Mandrel Test, 300 CPASSES CEE10/IIed
Needle Flame Test, 3.2 mm, Burn Time sPASSES IEC 60695-2-2
Water Absorption, 24 hours, mg8 DIN 53495

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.