MatWeb, The Online Materials Database

SABIC Innovative Plastics VALOX 508 PBT (Europe)


Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line. This product is also a part of their North American product line.

Physical PropertiesOriginal ValueComments
Density1.5 g/cc ASTM D 792
Density1.5 g/cc ISO 1183
Water Absorption0.06 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.06 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.09 % 23C; ISO 62
Linear Mold Shrinkage0.004 - 0.006 cm/cm Flow; ASTM D 955
Linear Mold Shrinkage, Transverse0.005 - 0.009 cm/cm ASTM D 955
Melt Flow8 g/10 min cm3/10min; Melt Volume Rate, MVR at 250C/2.16 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell R119 ISO 2039/2
Hardness, H358/30122 MPa ISO 2039/1
Tensile Strength, Ultimate110 MPa ASTM D 638
Tensile Strength, Ultimate115 MPa 5 mm/min; ISO 527
Elongation at Break2 % 5 mm/min; ISO 527
Elongation at Break3 % ASTM D 638
Tensile Modulus9 GPa 1 mm/min; ISO 527
Flexural Modulus6.9 GPa DIN 53457
Flexural Modulus8 GPa 2 mm/min; ISO 178
Flexural Strength170 MPa DIN 53452
Flexural Strength170 MPa 2 mm/min; ISO 178
Ultimate Compressive Strength115 MPa ASTM D 695
Shear Strength56 MPa ASTM D 732
Izod Impact, Notched1.05 J/cm 23 C; ASTM D 256
Izod Impact, Notched (ISO)8 kJ/m² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched (ISO)45 kJ/m² 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)40 kJ/m² 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp (ISO)7 kJ/m² 80*10*4 -30 C; ISO 180/ 1A
Charpy Impact Unnotched4.5 J/cm² 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched, Low Temp0.65 J/cm² at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Unnotched Low Temp4.5 J/cm² at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched0.75 J/cm² 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Taber Abrasion, mg/1000 Cycles50 CS-17, 1 kg; GE Test

Electrical Properties
Volume ResistivityMin 1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant3.2 1 MHz; IEC 60250
Dielectric Constant3.3 50 Hz; IEC 60250
Dielectric Constant3.6 100 Hz; IEC 60250
Dielectric Strength16 kV/mm in oil, 3.2 mm; IEC 60243-1
Dielectric Strength23 kV/mm in oil, 1.6 mm; IEC 60243-1
Dielectric Strength24 kV/mm Short time, 3.2 mm; ASTM D 149
Dielectric Strength24 kV/mm Short time, 1.0 mm; IEC 60243-1
Dielectric Strength30 kV/mm in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.001 50 Hz; IEC 60250
Dissipation Factor0.0014 100 Hz; IEC 60250
Dissipation Factor0.013 1 MHz; IEC 60250
Arc Resistance62 sec Tungsten; ASTM D 495
Comparative Tracking Index150 V M; IEC 60112/3rd
Comparative Tracking Index250 V IEC 60112/3rd
Comparative Tracking Index250 V Stand. Black; IEC 60112/3rd
Comparative Tracking Index275 V Electr Grey; IEC 60112/3rd
Hot Wire Ignition, HWI66 sec UL 746A
High Amp Arc Ignition, HAI15 arcs on surface; UL 746A
High Voltage Arc-Tracking Rate, HVTR1.8 mm/min UL 746A

Thermal Properties
CTE, linear 20°C25 µm/m-°C 23C-80C, flow; ISO 11359-2
CTE, linear 20°C Transverse to Flow100 µm/m-°C 23C-80C; ISO 11359-2
CTE, linear 100°C105 µm/m-°C 23C-150C, cross flow; ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi)206 °C HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 0.46 MPa (66 psi)215 °C ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)160 °C HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Deflection Temperature at 1.8 MPa (264 psi)175 °C ASTM D 648
Vicat Softening Point170 °C B/50; ISO 306
Vicat Softening Point175 °C B/120; ISO 306
Vicat Softening Point215 °C Rate B; ASTM D 1525
Vicat Softening Point217 °C A/50; ISO 306
UL RTI, Electrical125 °C UL 746B
UL RTI, Mechanical with Impact110 °C UL 746B
UL RTI, Mechanical without Impact125 °C UL 746B
Flammability, UL94HB 1.5 mm
Oxygen Index21 % ISO 4589
Glow Wire Test750 °C Passes at 1 mm; EDF HN60S02
Glow Wire Test750 °C Passes at 1 mm; IEC 60695-2-1

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.