MatWeb, The Online Materials Database

SABIC Innovative Plastics VALOX 865 PBT (Europe)


Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line. This product is also a part of their North American product line.

Physical PropertiesOriginal ValueComments
Density1.66 g/cc ASTM D 792
Density1.66 g/cc ISO 1183
Water Absorption0.03 % 24 hours; ASTM D 570
Moisture Absorption at Equilibrium0.03 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.32 % 23C; ISO 62
Linear Mold Shrinkage0.004 - 0.008 cm/cm Flow; ASTM D 955
Linear Mold Shrinkage, Transverse0.006 - 0.01 cm/cm ASTM D 955
Melt Flow7 g/10 min cm3/10min; Melt Volume Rate, MVR at 265C/1.2 kg; ISO 1133

Mechanical Properties
Hardness, Rockwell R119 ISO 2039/2
Hardness, H358/30130 MPa ISO 2039/1
Tensile Strength, Ultimate115 MPa ASTM D 638
Tensile Strength, Ultimate130 MPa 5 mm/min; ISO 527
Elongation at Break2 % 5 mm/min; ISO 527
Tensile Modulus10 GPa 1 mm/min; ISO 527
Flexural Modulus7.6 GPa DIN 53457
Flexural Modulus8 GPa 2 mm/min; ISO 178
Flexural Strength180 MPa DIN 53452
Flexural Strength195 MPa 2 mm/min; ISO 178
Izod Impact, Notched0.8 J/cm 23 C; ASTM D 256
Izod Impact, Notched (ISO)7 kJ/m² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched (ISO)55 kJ/m² 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)55 kJ/m² 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp (ISO)6 kJ/m² 80*10*4 -30 C; ISO 180/ 1A
Charpy Impact Unnotched5 J/cm² 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched, Low Temp0.8 J/cm² at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Unnotched Low TempNB at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched0.8 J/cm² 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA

Electrical Properties
Volume Resistivity1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant3.3 1 MHz; IEC 60250
Dielectric Constant3.4 50 Hz; IEC 60250
Dielectric Strength15 kV/mm in oil, 3.2 mm; IEC 60243-1
Dielectric Strength19 kV/mm in oil, 1.6 mm; IEC 60243-1
Dielectric Strength20 kV/mm Short time, 3.2 mm; ASTM D 149
Dielectric Strength22 kV/mm in oil, 0.8 mm; IEC 60243-1
Dissipation Factor0.001 50 Hz; IEC 60250
Dissipation Factor0.012 1 MHz; IEC 60250
Arc Resistance86 sec Tungsten; ASTM D 495
Comparative Tracking Index150 V M; IEC 60112/3rd
Comparative Tracking Index200 V Stand. Black; IEC 60112/3rd
Comparative Tracking Index225 V IEC 60112/3rd
Comparative Tracking Index225 V Electr Grey; IEC 60112/3rd
Hot Wire Ignition, HWI77 sec UL 746A
High Amp Arc Ignition, HAI16 arcs on surface; UL 746A
High Voltage Arc-Tracking Rate, HVTR11.5 mm/min UL 746A

Thermal Properties
CTE, linear 20°C35 µm/m-°C 23C-80C, flow; ISO 11359-2
CTE, linear 20°C Transverse to Flow100 µm/m-°C 23C-80C; ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi)212 °C ASTM D 648
Deflection Temperature at 0.46 MPa (66 psi)215 °C HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi)195 °C ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)197 °C HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point200 °C B/50; ISO 306
Vicat Softening Point200 °C B/120; ISO 306
Vicat Softening Point213 °C Rate B; ASTM D 1525
Vicat Softening Point220 °C A/50; ISO 306
UL RTI, Electrical110 °C UL 746B
UL RTI, Mechanical with Impact105 °C UL 746B
UL RTI, Mechanical without Impact110 °C UL 746B
Flammability, UL94V-0 1.5 mm
Flammability, UL947 94-3 mm
Flammability Test1 mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2
Oxygen Index31 % ISO 4589
Glow Wire Test960 °C Passes at 1 mm; EDF HN60S02
Glow Wire Test960 °C Passes at 1 mm; IEC 60695-2-1

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.