SABIC Innovative Plastics ULTEM® 6601 Polyetherimide, 5% Glass Filled, Injection Grade


Subcategory: Filled/Reinforced Thermoplastic; Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Data for 3.2 mm (1/8 in) samples unless otherwise noted. Data provided by GE Plastics.

Physical PropertiesOriginal ValueComments
Density1.32 g/cc ASTM D792
Melt Flow11 g/10 min 365°C/6.6kg; ASTM D1238

Mechanical Properties
Tensile Strength, Ultimate96 MPa ASTM D638
Elongation at Break15 % ASTM D638
Modulus of Elasticity3.7 GPa ASTM D638
Flexural Modulus4 GPa 6.4 mm sample; ASTM D790
Flexural Yield Strength176 MPa ASTM D790

Thermal Properties
Deflection Temperature at 1.8 MPa (264 psi)215 °C 6.4 mm (0.25 in.) sample; ASTM D648

Processing Properties
Processing Temperature382 - 404 °C Suggested injection molding melt temperature
Mold Temperature135 - 162 °C 
Drying Temperature149 °C 
Dry Time4 - 6 hour 24 hr Max.

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.