SABIC Innovative Plastics ULTEM® CRS5011F Polyetherimide, Unfilled, Injection/Extrusion Grade


Subcategory: Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Data for 3.2 mm (1/8 in) samples unless otherwise noted. Data provided by GE Plastics.

Physical PropertiesOriginal ValueComments
Density1.28 g/cc ASTM D792
Linear Mold Shrinkage0.004 - 0.007 cm/cm 3.2 mm sample
Melt Flow10.8 g/10 min 335°C/6.6kg; ASTM D1238

Mechanical Properties
Tensile Strength, Ultimate100 MPa ASTM D638
Elongation at Break70 % ASTM D638
Modulus of Elasticity2.9 GPa ASTM D638
Flexural Modulus3.1 GPa 6.4 mm sample; ASTM D790
Flexural Yield Strength138 MPa ASTM D790
Izod Impact, Notched0.3 J/cm 3.2 mm sample; ASTM D256

Thermal Properties
Deflection Temperature at 1.8 MPa (264 psi)204 °C 6.4 mm (0.25 in.) sample; ASTM D648

Processing Properties
Processing Temperature365 - 387 °C Suggested injection molding melt temperature
Mold Temperature135 - 162 °C 
Drying Temperature149 °C 
Dry Time4 - 6 hour 24 hr Max.

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.