MatWeb, The Online Materials Database
SABIC Innovative Plastics VALOX® 469 PBT, 30% Glass Filled, Injection Grade
Subcategory: Filled/Reinforced Thermoplastic; Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Data for 3.2 mm (1/8 in) samples unless otherwise noted. Data provided by GE Plastics.
Physical Properties | Original Value | Comments |
|
Density | 1.65 g/cc | ASTM D792 |
Water Absorption | 0.06 % | 24 hrs; 20°C; ASTM D570 |
Linear Mold Shrinkage | 0.005 - 0.008 cm/cm | 6.4 mm sample |
Linear Mold Shrinkage | 0.003 - 0.005 cm/cm | 3.2 mm sample |
Mechanical Properties |
|
Tensile Strength, Ultimate | 96 MPa | ASTM D638 |
Flexural Modulus | 6.9 GPa | 3.2 mm sample; ASTM D790 |
Izod Impact, Notched | 0.5 J/cm | 3.2 mm sample; ASTM D256 |
Electrical Properties |
|
Electrical Resistivity | 2e+016 ohm-cm | ASTM D257 |
Thermal Properties |
|
Deflection Temperature at 1.8 MPa (264 psi) | 187 °C | 6.4 mm (0.25 in.) sample; ASTM D648 |
UL RTI, Electrical | 120 °C | UL 746B |
UL RTI, Mechanical with Impact | 120 °C | UL 746B |
UL RTI, Mechanical without Impact | 120 °C | UL 746B |
Flammability, UL94 | V-0 | 5V at 2.5 mm. |
Flammability, UL94 | V-0 | 1.4 mm |
Processing Properties |
|
Processing Temperature | 248 - 265 °C | Suggested injection molding melt temperature |
Mold Temperature | 65 - 87 °C | |
Drying Temperature | 121 °C | |
Dry Time | 3 - 4 hour | 12 hrs Max |
|
|
|
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
|