EMS-Grivory Grilon® FE 8023 Natural Nylon 6, Dry As Molded
Subcategory: Nylon; Nylon 6; Polymer; Thermoplastic
Material Notes: Grilon FE 8023 natural is a new heat stabilized injection molding grade based on Polyamide 6.Information provided by EMS-Grivory
Physical Properties | Original Value | Comments |
|
Density | 1.15 g/cc | ISO 1183 |
Linear Mold Shrinkage | 0.009 cm/cm | ISO 294 |
Linear Mold Shrinkage, Transverse | 0.006 cm/cm | ISO 294 |
Melt Flow | 57.5 g/10 min | 275°C / 5kg; ISO 11133 |
Mechanical Properties |
|
Tensile Strength at Break | 100 MPa | 5 mm/min; ISO 527 |
Elongation at Break | 3 % | 5 mm/min; ISO 527 |
Tensile Modulus | 4.6 GPa | 1 mm/min; ISO 527 |
Charpy Impact Unnotched | 7 J/cm² | ISO 179/1eU |
Charpy Impact, Notched, Low Temp | 0.4 J/cm² | -30°C; ISO 179/1eA |
Charpy Impact, Unnotched Low Temp | 6.5 J/cm² | -30°C; ISO 179/1eU |
Charpy Impact, Notched | 0.4 J/cm² | ISO 179/1eA |
Thermal Properties |
|
Melting Point | 220 °C | ISO 11357 |
Deflection Temperature at 0.46 MPa (66 psi) | 180 °C | ISO 75 |
Deflection Temperature at 1.8 MPa (264 psi) | 100 °C | ISO 75 |
Processing Properties |
|
Melt Temperature | 240 - 300 °C | Injection molding |
Mold Temperature | 80 - 100 °C | Injection molding |
Hold Pressure | 50 - 75 MPa | |
Back Pressure | 0.5 - 1.5 MPa | |
Screw Speed | 50 - 100 rpm | |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |