PolyOne Geon® 87150 Vinyl Compound - Rigid (RPVC)


Subcategory: Polymer; Thermoplastic; Vinyl

Material Notes:

Description/Features:

  • Interior
  • High HDT
  • UL 94 5VA
  • UL 94 V0
  • CSA V0
  • CSA 5VA
  • NSF STD 51

Applications:

  • Custom Profiles

Processing Method:

  • Extrusion-Single Screw

Disclaimer: Note: NSF listings are obtained on specific colors. Contact PolyOne for the latest listing of approved colors for this product.
Note: The Cell Classification was determined using the notched Izod test with injection molded samples.

Information provided by PolyOne Corporation.

Physical PropertiesMetricEnglishComments
Specific Gravity1.44 g/cc0.052 lb/in³ ASTM D792

Mechanical Properties
Hardness, Shore D82.982.9 15 sec; ASTM D2240
Tensile Strength, Yield41.9 MPa6080 psi Type 1 - Rigids, 0.2 in/min; ASTM D638
Tensile Modulus2.71 GPa392.4 ksi Type 1 - Rigids, 0.2 in/min; ASTM D638
Flexural Modulus2.52 GPa366 ksi ASTM D790
Flexural Strength72.1 MPa10450 psi ASTM D790
Dart Drop Total Energy53.4 J/cm0.1 ft-lb/mil Procedure A, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Dart Drop Total Energy107 J/cm0.2 ft-lb/mil Procedure B, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Izod Impact, Notched6.99 J/cm13.1 ft-lb/in Method A, With Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched8.7 J/cm16.3 ft-lb/in Method A, Against Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched10.9 J/cm20.5 ft-lb/in Method A, Injection Molded, 0.125 in bars, 73°F (23°C); ASTM D256

Thermal Properties
CTE, linear 68°F64.8 µm/m-°C36 µin/in-°F ASTM D696
Deflection Temperature at 1.8 MPa (264 psi)74.4 °C166 °F Unannealed, 0.125 in bars; ASTM D648
Flammability, UL94V-0V-0 All Colors; 0.028 in.
Flammability, UL94V-0V-0 All Colors; 0.03 in.
Flammability, UL9477 All Colors; 0.029 in.
Flammability, UL9477 All Colors; 0.075 in.

Processing Properties
Melt Temperature182 - 193 °C360 - 380 °F Extrusion

Descriptive Properties
Cell Classification D178416344 ASTM D1784
Ease of SizingGood 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.