MatWeb, The Online Materials Database

PolyOne Geon® 87263 Vinyl Compound - Rigid (RPVC)


Subcategory: Polymer; Thermoplastic; Vinyl

Material Notes:

Description/Features:

  • Exterior-Weatherable Natural Base
  • UL 94 V0

Applications:

  • Custom Profiles

Processing Method:

  • Extrusion-Single Screw
PolyOne First Choice

Disclaimer: NOTE: Geon weatherable compounds contain pigments and ingredients that, along with processing conditions, contribute to the weathering performance of the PVC compounds. The weathering performance of unpigmented compounds or so-called natural compounds generally is inferior to pigmented compounds. Unpigmented weatherable compounds may also contain non-pigment ingredients which can interact unpredictably with pigments to produce unexpected weathering results. Therefore, in applications where processors or customers would like to use an unpigmented compound, or add their own pigment package, it is the customer’s responsibility to determine whether or not the weathering performance after pigmenting is acceptable in their specific end-use application.
Note: The Cell Classification was determined using the notched Izod test with injection molded samples.

Information provided by PolyOne Corporation.

Physical PropertiesOriginal ValueComments
Specific Gravity1.4 g/cc ASTM D792

Mechanical Properties
Hardness, Shore D82.3 15 sec; ASTM D2240
Tensile Strength, Yield6850 psi Type 1 - Rigids, 0.2 in/min; ASTM D638
Tensile Modulus420500 psi Type 1 - Rigids, 0.2 in/min; ASTM D638
Flexural Modulus411 ksi ASTM D790
Flexural Strength12190 psi ASTM D790
Dart Drop Total Energy0.11 ft-lb/mil Procedure A, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Dart Drop Total Energy0.11 ft-lb/mil Procedure B, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Izod Impact, Notched18.4 ft-lb/in Method A, With Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched20 ft-lb/in Method A, Against Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched20.2 ft-lb/in Method A, Injection Molded, 0.125 in bars, 73°F (23°C); ASTM D256

Thermal Properties
CTE, linear 68°F36 µin/in-°F ASTM D696
Deflection Temperature at 1.8 MPa (264 psi)163 °F Unannealed, 0.125 in bars; ASTM D648

Processing Properties
Melt Temperature360 - 380 °F 

Descriptive Properties
Cell Classification D178416354 ASTM D1784
Cell Classification D421614143431 ASTM D4216
Ease of SizingGood 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.