Material Notes:

Description/Features:

  • Interior
  • Chemical Resistant
  • NSF Type I
  • NSF STD 14
  • NSF STD 61

Applications:

  • Pipe-Pressure

Processing Method:

  • Extrusion-Single Screw

Disclaimer: Note: NSF listings are obtained on specific colors. Contact PolyOne for the latest listing of approved colors for this product.

Information provided by PolyOne Corporation.

Physical PropertiesMetricEnglishComments
Specific Gravity1.4 g/cc0.0506 lb/in³ ASTM D792

Mechanical Properties
Hardness, Shore D8080 15 sec; ASTM D2240
Tensile Strength, Yield49 MPa7100 psi Type 1 - Rigids, 0.2 in/min; ASTM D638
Tensile Modulus2.99 GPa433 ksi Type 1 - Rigids, 0.2 in/min; ASTM D638
Flexural Modulus3.19 GPa462 ksi ASTM D790
Flexural Strength98.6 MPa14300 psi ASTM D790
Dart Drop Total Energy69.4 J/cm0.13 ft-lb/mil Procedure A, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Dart Drop Total Energy198 J/cm0.37 ft-lb/mil Procedure B, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Izod Impact, Notched0.587 J/cm1.1 ft-lb/in Method A, With Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched0.641 J/cm1.2 ft-lb/in Method A, Against Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched0.801 J/cm1.5 ft-lb/in Method A, Injection Molded, 0.125 in bars, 73°F (23°C); ASTM D256

Thermal Properties
CTE, linear 68°F61.2 µm/m-°C34 µin/in-°F ASTM D696
Deflection Temperature at 1.8 MPa (264 psi)75.6 °C168 °F Unannealed, 0.125 in bars; ASTM D648

Processing Properties
Melt Temperature182 - 193 °C360 - 380 °F Extrusion

Descriptive Properties
Cell Classification D178413454 ASTM D1784
Ease of SizingGood 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.