MatWeb, The Online Materials Database

PolyOne Geon® 87549 Vinyl Compound - Rigid (RPVC)


Subcategory: Polymer; Thermoplastic; Vinyl

Material Notes:

Description/Features:

  • Transparent
  • Interior
  • UL 94 V0

Applications:

  • Custom Profiles
  • Point of Purchase Datastrips

Processing Method:

  • Extrusion-Profile

Disclaimer: Note: The Cell Classification was determined using the notched Izod test with injection molded samples.

Information provided by PolyOne Corporation.

Physical PropertiesMetricEnglishComments
Specific Gravity1.34 g/cc0.0484 lb/in³ ASTM D792

Mechanical Properties
Hardness, Shore D8585 15 sec; ASTM D2240
Tensile Strength, Yield41.4 MPa6000 psi Type 1 - Rigids, 0.2 in/min; ASTM D638
Tensile Modulus2.48 GPa360 ksi Type 1 - Rigids, 0.2 in/min; ASTM D638
Flexural Modulus2.9 GPa420 ksi ASTM D790
Flexural Strength91.9 MPa13330 psi ASTM D790
Dart Drop Total Energy64.1 J/cm0.12 ft-lb/mil Procedure A, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Dart Drop Total Energy171 J/cm0.32 ft-lb/mil Procedure B, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Izod Impact, Notched0.908 J/cm1.7 ft-lb/in Method A, With Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched10.9 J/cm20.4 ft-lb/in Method A, Injection Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched5.18 J/cm9.7 ft-lb/in Method A, Against Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256

Thermal Properties
CTE, linear 68°F70.2 µm/m-°C39 µin/in-°F ASTM D696
Deflection Temperature at 1.8 MPa (264 psi)71.1 °C160 °F Unannealed, 0.125 in bars; ASTM D648

Processing Properties
Melt Temperature182 - 193 °C360 - 380 °F 

Descriptive Properties
Cell Classification D178416354 ASTM D1784

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.