MatWeb, The Online Materials Database

PolyOne Geon® 87775 Vinyl Compound - Rigid (RPVC)


Subcategory: Polymer; Thermoplastic; Vinyl

Material Notes:

Description/Features:

  • Exterior-Weatherable
  • AAMA 303

Applications:

  • Custom Profiles
  • Window Components

Market:

  • Windows
  • Doors

Processing Method:

  • Extrusion-Profile

Disclaimer: Note: The Cell Classification was determined using the notched Izod test with injection molded samples.

Information provided by PolyOne Corporation.

Physical PropertiesMetricEnglishComments
Specific Gravity1.45 g/cc0.0524 lb/in³ ASTM D792

Mechanical Properties
Hardness, Shore D7878 15 sec; ASTM D2240
Tensile Strength, Yield44.5 MPa6460 psi Type 1 - Rigids, 0.2 in/min; ASTM D638
Tensile Modulus2.76 GPa400 ksi Type 1 - Rigids, 0.2 in/min; ASTM D638
Flexural Modulus2.74 GPa398 ksi ASTM D790
Flexural Strength80 MPa11600 psi ASTM D790
Dart Drop Total Energy58.7 J/cm0.11 ft-lb/mil Procedure A, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Dart Drop Total Energy58.7 J/cm0.11 ft-lb/mil Procedure B, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Izod Impact, Notched1.23 J/cm2.3 ft-lb/in Method A, Against Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched13.6 J/cm25.4 ft-lb/in Method A, Injection Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched1.71 J/cm3.2 ft-lb/in Method A, With Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256

Thermal Properties
CTE, linear 68°F68.4 µm/m-°C38 µin/in-°F ASTM D696
Deflection Temperature at 1.8 MPa (264 psi)71.1 °C160 °F Unannealed, 0.125 in bars; ASTM D648

Processing Properties
Melt Temperature182 - 193 °C360 - 380 °F 

Descriptive Properties
Cell Classification D421614113333 ASTM D4216
Ease of SizingGood 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.