MatWeb, The Online Materials Database

PolyOne Geon® 87850 Vinyl Compound - Rigid (RPVC)


Subcategory: Polymer; Thermoplastic; Vinyl

Material Notes:

Description/Features:

  • Exterior-Weatherable

Applications:

  • General Purpose

Processing Method:

  • Extrusion-Sheet
PolyOne First Choice

Disclaimer: Note: The Cell Classification was determined using the notched Izod test with injection molded samples.

Information provided by PolyOne Corporation.

Physical PropertiesOriginal ValueComments
Specific Gravity1.44 g/cc ASTM D792

Mechanical Properties
Hardness, Shore D82.2 15 sec; ASTM D2240
Tensile Strength, Yield6290 psi Type 1 - Rigids, 0.2 in/min; ASTM D638
Tensile Modulus360000 psi Type 1 - Rigids, 0.2 in/min; ASTM D638
Flexural Modulus10 ksi ASTM D790
Flexural Strength35500 psi ASTM D790
Dart Drop Total Energy0.12 ft-lb/mil Procedure A, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Dart Drop Total Energy0.24 ft-lb/mil Procedure B, 0.125 in Conical Dart, 73°F (23°C); ASTM D4226
Izod Impact, Notched11.8 ft-lb/in Method A, Injection Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched13.5 ft-lb/in Method A, With Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256
Izod Impact, Notched16.4 ft-lb/in Method A, Against Grain - Comp. Molded, 0.125 in bars, 73°F (23°C); ASTM D256

Thermal Properties
CTE, linear 68°F40.5 µin/in-°F ASTM D696
Deflection Temperature at 1.8 MPa (264 psi)154 °F Unannealed, 0.125 in bars; ASTM D648

Processing Properties
Melt Temperature370 - 400 °F Extrusion

Descriptive Properties
Cell Classification D178415343 ASTM D1784
Cell Classification D421614133223 ASTM D4216

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.