PolyOne Geon® 90042 Vinyl Compound - Flexible (FPVC)


Subcategory: Polymer; Thermoplastic; Vinyl

Material Notes:

Description/Features:

  • Exterior
  • Low Gloss

Applications:

  • Beltline Moldings
  • Greenhouse Trim

Market:

  • Automotive

Processing Method:

  • Extrusion

Disclaimer: Note: Automotive OEM approval(s).

Information provided by PolyOne Corporation.

Physical PropertiesOriginal ValueComments
Specific Gravity1.3 g/cc ASTM D792
Collected Volatile Condensable Material0.32 % Method A, 221°F (105°C), 0.075 in; ASTM D1203B

Mechanical Properties
Hardness, Shore A79 15 sec; ASTM D2240
Tensile Strength, Ultimate2828 psi 20 in/min; ASTM D638
Elongation at Break304 % 20 in/min; ASTM D638
Tear Strength388 pli Die C (graves), 2 in/min; ASTM D1004

Descriptive Properties
Automotive ApprovalGeneral Motors, GMP.PVC.007 
Fungal ResistancePass ASTM G21
Low Temperature Flexibility (LTF)Pass 12 mm, -20°F (-29°C), 4 hrs, 0.020 in
Product FormPellets 
Xenon Weatherometer - ExteriorPass 2,500 kJ/m², Black, dE*; SAE J1960

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.