Physical PropertiesOriginal ValueComments
Density1.02 g/cc 
Water Absorption1 % 
Moisture Absorption at EquilibriumMax 0.5 % Humidity Absorption
Melt Flow120 g/10 min 

Mechanical Properties
Tensile Strength, Yield45 MPa 
Elongation at BreakMin 50 % 
Elongation at Yield5 % 
Modulus of Elasticity1.4 GPa 
Charpy Impact UnnotchedNB 
Charpy Impact, Notched, Low Temp0.8 J/cm² at -30°C
Charpy Impact, Unnotched Low TempNB at -30°C
Charpy Impact, Notched0.6 J/cm² 
Tensile Creep Modulus, 1 hour1000 MPa 
Tensile Creep Modulus, 1000 hours700 MPa 

Electrical Properties
Electrical ResistivityMin 1e+015 ohm-cm 
Surface ResistanceMin 1e+015 ohm 
Dielectric Constant2 at 1 MHz.
Dielectric Constant, Low Frequency3 100 Hz
Dielectric Strength26 kV/mm 
Dissipation Factor0.028 at 1 MHz.
Dissipation Factor, Low Frequency0.031 100 Hz
Comparative Tracking Index600 V 

Thermal Properties
CTE, linear 20°C100 µm/m-°C in flow direction.
CTE, linear 20°C Transverse to Flow100 µm/m-°C 
Deflection Temperature at 0.46 MPa (66 psi)110 °C 
Deflection Temperature at 1.8 MPa (264 psi)50 °C 
Vicat Softening Point140 °C 50°C/hr/50 N
Flammability, UL94HB 1.6 mm
Flammability, UL94HB 3.2 mm

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.