MatWeb, The Online Materials Database
Degussa AG VESTAMID® L2123 sw 9.7507 (as-conditioned) Nylon 12
Subcategory: Nylon; Nylon 12; Polymer; Thermoplastic
Close Analogs: This former Creanova product line is a part of Degussa AG as of 2001.
Key Words: Polyamide
Material Notes: ISO data as provided by the manufacturer, Creanova, Inc. Uses: Flexible tubing for the automobile industry.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.03 g/cc | 0.0372 lb/in³ | |
| Moisture Absorption at Equilibrium | Max 0.5 % | Max 0.5 % | Humidity Absorption |
Mechanical Properties |
|
| Tensile Strength, Yield | 25 MPa | 3630 psi | |
| Elongation at Break | Min 50 % | Min 50 % | |
| Elongation at Yield | 30 % | 30 % | |
| Modulus of Elasticity | 0.4 GPa | 58 ksi | |
| Charpy Impact Unnotched | NB | NB | |
| Charpy Impact, Notched, Low Temp | 0.8 J/cm² | 3.81 ft-lb/in² | at -30°C |
| Charpy Impact, Unnotched Low Temp | NB | NB | at -30°C |
| Charpy Impact, Notched | NB | NB | |
Electrical Properties |
|
| Electrical Resistivity | 7e+010 ohm-cm | 7e+010 ohm-cm | |
| Surface Resistance | 2e+012 ohm | 2e+012 ohm | |
| Dielectric Constant | 4 | 4 | at 1 MHz. |
| Dielectric Constant, Low Frequency | 15 | 15 | 100 Hz |
| Dielectric Strength | 33 kV/mm | 838 kV/in | |
| Dissipation Factor | 0.14 | 0.14 | at 1 MHz. |
| Dissipation Factor, Low Frequency | 0.33 | 0.33 | 100 Hz |
Thermal Properties |
|
| CTE, linear 20°C | Max 50 µm/m-°C | Max 27.8 µin/in-°F | |
| Deflection Temperature at 0.46 MPa (66 psi) | 90 °C | 194 °F | |
| Deflection Temperature at 1.8 MPa (264 psi) | 45 °C | 113 °F | |
| Vicat Softening Point | 120 °C | 248 °F | 50°C/hr/50 N |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |