Physical Properties | Metric | English | Comments |
|
Density | 1.23 g/cc | 0.0444 lb/in³ | |
Water Absorption | 2 % | 2 % | |
Melt Flow | 10 g/10 min | 10 g/10 min | |
Mechanical Properties |
|
Tensile Strength, Ultimate | 130 MPa | 18900 psi | |
Elongation at Break | 5 % | 5 % | |
Modulus of Elasticity | 5.5 GPa | 798 ksi | |
Charpy Impact Unnotched | 8 J/cm² | 38.1 ft-lb/in² | |
Charpy Impact, Notched, Low Temp | 0.7 J/cm² | 3.33 ft-lb/in² | at -30°C |
Charpy Impact, Unnotched Low Temp | 2 J/cm² | 9.52 ft-lb/in² | at -30°C |
Charpy Impact, Notched | 1.2 J/cm² | 5.71 ft-lb/in² | |
Electrical Properties |
|
Electrical Resistivity | Min 1e+015 ohm-cm | Min 1e+015 ohm-cm | |
Surface Resistance | Min 1e+015 ohm | Min 1e+015 ohm | |
Dielectric Constant | 4 | 4 | 100 Hz |
Dielectric Constant, Low Frequency | 4 | 4 | 100 Hz |
Dielectric Strength | 38 kV/mm | 965 kV/in | |
Thermal Properties |
|
CTE, linear 20°C | Max 50 µm/m-°C | Max 27.8 µin/in-°F | |
Deflection Temperature at 0.46 MPa (66 psi) | 210 °C | 410 °F | |
Deflection Temperature at 1.8 MPa (264 psi) | 190 °C | 374 °F | |
Vicat Softening Point | 205 °C | 401 °F | 50°C/hr/50 N |
Flammability, UL94 | HB | HB | 1.6 mm |
Flammability, UL94 | HB | HB | 3.2 mm |
|
|
|
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
|