Degussa AG Vestamid® D16 Nylon 612 (Dry as Molded)


Subcategory: Nylon; Nylon 612; Polymer; Thermoplastic

Key Words: PA612, LN, 12-020

Material Notes:
Description: low-viscosity base product

Applications: monofilaments, bristles with high recovery for paint brushes and tooth brushes

Information provided by degussa.

Physical PropertiesOriginal ValueComments
Density1.06 g/cc ISO 1183
Moisture Absorption at Equilibrium1 % 23°C/50% R.H.; ISO 62
Water Absorption at Saturation2.6 % ISO 62
Linear Mold Shrinkage0.014 cm/cm 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2)
Linear Mold Shrinkage, Transverse0.01 cm/cm 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2)

Mechanical Properties
Tensile Strength, Yield58 MPa ISO 527-2/1A
Elongation at BreakMin 50 % ISO 527-2/1A
Elongation at Yield5 % ISO 527-2/1A
Tensile Modulus2 GPa ISO 527-2/1A
Charpy Impact UnnotchedNB 23°C; ISO 179/1eU
Charpy Impact, Notched, Low Temp0.6 J/cm² -30°C; ISO 179/1eA
Charpy Impact, Unnotched Low TempNB -30°C; ISO 179/1eU
Charpy Impact, Notched0.5 J/cm² 23°C; ISO 179/1eA

Electrical Properties
Volume Resistivity1e+015 ohm-cm IEC 60093
Dielectric Constant3.2 23°C/1 MHz; IEC 60250
Dielectric Constant, Low Frequency3.8 23°C/100 Hz; IEC 60250
Dielectric Strength28 kV/mm K20/P50; IEC 60243-1
Dissipation Factor0.029 23°C/1 MHz; IEC 60250
Dissipation Factor, Low Frequency0.024 23°C/100 Hz; IEC 60250
Comparative Tracking IndexMin 600 V Test Solution A, 100 drops; IEC 60112

Thermal Properties
CTE, linear 20°C130 µm/m-°C 23-55°C ; ISO 11359
Melting Point215 °C Peak Temperature; ISO 3146, ISO 11357
Deflection Temperature at 0.46 MPa (66 psi)150 °C ISO 75
Deflection Temperature at 1.8 MPa (264 psi)65 °C ISO 75
Deflection Temperature at 1.8 MPa (264 psi)75 °C When conditioned at 180°C for 1 hour; ISO 75
Vicat Softening Point180 °C 50N; ISO 306
Flammability, UL94HB 3.2 mm
Flammability, UL94HB 1.6 mm

Descriptive Properties
Electrolytic CorrosionA1 Step IEC 60426

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.