MatWeb, The Online Materials Database

Degussa AG Vestamid® DX9301 Black Nylon 612 with 4% Graphite (Dry as Molded)


Subcategory: Filled/Reinforced Thermoplastic; Nylon; Nylon 612; Polymer; Thermoplastic

Key Words: PA612, MHR, 14-030, CD04

Material Notes:
Description: medium-viscosity, heat-stabilized, similar to X7094, but suffers less wear from abrasion

Applications: components exposed to friction

Information provided by degussa.

Physical PropertiesMetricEnglishComments
Density1.09 g/cc0.0394 lb/in³ ISO 1183
Moisture Absorption at Equilibrium1 %1 % 23°C/50% R.H.; ISO 62
Water Absorption at Saturation2.7 %2.7 % ISO 62
Linear Mold Shrinkage0.012 cm/cm0.012 in/in 127x12.7x3.2 mm (processing cond. acc. To DIN EN ISO 1874-2)
Linear Mold Shrinkage, Transverse0.014 cm/cm0.014 in/in 127x12.7x3.2 mm (processing cond. acc. To DIN EN ISO 1874-2)

Mechanical Properties
Tensile Strength at Break65 MPa9430 psi ISO 527-2/1A
Elongation at Break7 %7 % ISO 527-2/1A
Tensile Modulus2.65 GPa384 ksi ISO 527-2/1A
Charpy Impact Unnotched11.5 J/cm²54.7 ft-lb/in² 23°C; ISO 179/1eU
Charpy Impact, Notched, Low Temp0.3 J/cm²1.43 ft-lb/in² -30°C; ISO 179/1eA
Charpy Impact, Unnotched Low Temp11 J/cm²52.4 ft-lb/in² -30°C; ISO 179/1eU
Charpy Impact, Notched0.4 J/cm²1.9 ft-lb/in² 23°C; ISO 179/1eA

Thermal Properties
CTE, linear 20°C110 µm/m-°C61.1 µin/in-°F 23-55°C, Transverse; ISO 11359
CTE, linear 20°C130 µm/m-°C72.2 µin/in-°F 23-55°C, Longitudinal; ISO 11359
Melting Point215 °C419 °F Peak Temperature; ISO 11357
Deflection Temperature at 0.46 MPa (66 psi)185 °C365 °F ISO 75
Deflection Temperature at 1.8 MPa (264 psi)85 °C185 °F ISO 75
Vicat Softening Point187 °C369 °F 50N; ISO 306

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.