MatWeb, The Online Materials Database
Degussa AG Vestamid® L2123 Plasticized Nylon 12
Subcategory: Nylon; Nylon 12; Polymer; Thermoplastic
Key Words: PA12-P, EHL,22-004
Material Notes: Description: High-viscosity, plasticized, heat- and light-stabilized, with processing aid, increased low-temperature impact strength Applications: Tubing and coils for air brake lines, with high cold impact strength, meets SAE J844, ISO 7628, and DIN 74323/74324 Information provided by degussa.
Physical Properties | Original Value | Comments |
|
Density | 1.03 g/cc | ISO 1183 |
Moisture Absorption at Equilibrium | 0.6 % | 23°C/50% R.H. (1mm); ISO 62 |
Linear Mold Shrinkage | 0.012 cm/cm | 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2) |
Linear Mold Shrinkage, Transverse | 0.015 cm/cm | 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2) |
Mechanical Properties |
|
Tensile Strength, Yield | 24 MPa | ISO 527-1/2 |
Elongation at Break | Min 50 % | ISO 527-1/2 |
Elongation at Yield | 32 % | ISO 527-1/2 |
Tensile Modulus | 0.37 GPa | ISO 527-1/2 |
Charpy Impact Unnotched | NB | 23°C; ISO 179/1eU |
Charpy Impact, Notched, Low Temp | 1.3 J/cm² | -30°C; ISO 179/1eA |
Charpy Impact, Unnotched Low Temp | NB | -30°C; ISO 179/1eU |
Charpy Impact, Notched | 11.5 J/cm² | 23°C, Partial Break; ISO 179/1eA |
Electrical Properties |
|
Volume Resistivity | 1e+012 ohm-cm | IEC 60093 |
Dielectric Constant | 3.6 | 23°C/1 MHz; IEC 60250 |
Dielectric Constant, Low Frequency | 10 | 23°C/100 Hz; IEC 60250 |
Dielectric Strength | 29 kV/mm | K20/P50; IEC 60243-1 |
Dissipation Factor | 0.11 | 23°C/1 MHz; IEC 60250 |
Dissipation Factor, Low Frequency | 0.2 | 23°C/100 Hz; IEC 60250 |
Comparative Tracking Index | Min 600 V | Test Solution A, 50 drops; IEC 60112 |
Comparative Tracking Index | 600 V | Test Solution A, 100 drops; IEC 60112 |
Thermal Properties |
|
CTE, linear 20°C | 180 µm/m-°C | 23-55°C (45x15x10 mm); ISO 11359 |
Melting Point | 171 °C | Peak Temperature; ISO 3146, ISO 11357 |
Deflection Temperature at 0.46 MPa (66 psi) | 80 °C | ISO 75 |
Deflection Temperature at 1.8 MPa (264 psi) | 45 °C | ISO 75 |
Vicat Softening Point | 120 °C | 50N; ISO 306 |
Vicat Softening Point | 165 °C | 10N; ISO 306 |
Flammability, UL94 | HB | 3.2 mm |
Flammability, UL94 | HB | 1.6 mm |
Descriptive Properties | |
Color | Black | |
Electrolytic Corrosion | A1 Step | IEC 60426 |
|
|
|
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
|