MatWeb, The Online Materials Database

Degussa AG Vestamid® X7229 Flame Retardant Nylon 12


Subcategory: Nylon; Nylon 12; Polymer; Thermoplastic

Key Words: PA12-P, EFH,22-010

Material Notes:
Description: Plasticized, high-viscosity resin with flame retardant, free of halogen and phosphorus, UL 94-V2, meets FAR 25.853b

Applications: Profiles, tubes

Information provided by degussa.

Physical PropertiesMetricEnglishComments
Density1.06 g/cc0.0383 lb/in³ ISO 1183
Moisture Absorption at Equilibrium0.6 %0.6 % 23°C/50% R.H. (1mm); ISO 62
Water Absorption at Saturation1.5 %1.5 % 1 mm; ISO 62
Linear Mold Shrinkage0.011 cm/cm0.011 in/in 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2)
Linear Mold Shrinkage, Transverse0.012 cm/cm0.012 in/in 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2)

Mechanical Properties
Tensile Strength, Yield36 MPa5220 psi ISO 527-1/2
Elongation at BreakMin 50 %Min 50 % ISO 527-1/2
Elongation at Yield17 %17 % ISO 527-1/2
Tensile Modulus1 GPa145 ksi ISO 527-1/2
Charpy Impact UnnotchedNBNB 23°C; ISO 179/1eU
Charpy Impact, Notched, Low Temp0.5 J/cm²2.38 ft-lb/in² -30°C; ISO 179/1eA
Charpy Impact, Unnotched Low TempNBNB -30°C; ISO 179/1eU
Charpy Impact, Notched1.1 J/cm²5.24 ft-lb/in² 23°C; ISO 179/1eA

Electrical Properties
Volume Resistivity1e+013 ohm-cm1e+013 ohm-cm IEC 60093
Dielectric Constant55 23°C/1 MHz; IEC 60250
Dielectric Strength27 kV/mm686 kV/in K20/P50; IEC 60243-1
Dissipation Factor0.170.17 23°C/1 MHz; IEC 60250
Comparative Tracking IndexMin 600 VMin 600 V Test Solution A, 50 drops; IEC 60112
Comparative Tracking Index600 V600 V Test Solution A, 100 drops; IEC 60112

Thermal Properties
CTE, linear 20°C80 µm/m-°C44.4 µin/in-°F 23-55°C (45x15x10 mm); ISO 11359
Melting Point175 °C347 °F Peak Temperature; ISO 3146, ISO 11357
Deflection Temperature at 0.46 MPa (66 psi)130 °C266 °F ISO 75
Deflection Temperature at 1.8 MPa (264 psi)40 °C104 °F ISO 75
Vicat Softening Point150 °C302 °F 50N; ISO 306
Vicat Softening Point170 °C338 °F 10N; ISO 306
Flammability, UL94V-2V-2 3.2 mm
Flammability, UL94V-2V-2 1.6 mm

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.