Degussa AG Vestamid® X7293 Plasticized Nylon 12
Subcategory: Nylon; Nylon 12; Polymer; Thermoplastic
Key Words: PA12-HIP, EHL,22-004
Material Notes: Description: High-viscosity, plasticized, heat- and light-stabilized, with processing aid, increased low-temperature impact strength Applications: Fuel, vacuum and hydraulic lines; tubing for air brake lines, meets DIN 73378, 74324, ISO 7628, SAE J844 Information provided by degussa.
Physical Properties | Metric | English | Comments |
|
Density | 1.02 g/cc | 0.0368 lb/in³ | ISO 1183 |
Moisture Absorption at Equilibrium | 0.5 % | 0.5 % | 23°C/50% R.H. (1mm); ISO 62 |
Linear Mold Shrinkage | 0.013 cm/cm | 0.013 in/in | 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2) |
Linear Mold Shrinkage, Transverse | 0.014 cm/cm | 0.014 in/in | 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2) |
Mechanical Properties |
|
Tensile Strength, Yield | 27 MPa | 3920 psi | ISO 527-1/2 |
Elongation at Break | Min 50 % | Min 50 % | ISO 527-1/2 |
Elongation at Yield | 32 % | 32 % | ISO 527-1/2 |
Tensile Modulus | 0.4 GPa | 58 ksi | ISO 527-1/2 |
Charpy Impact Unnotched | NB | NB | 23°C; ISO 179/1eU |
Charpy Impact, Notched, Low Temp | 0.7 J/cm² | 3.33 ft-lb/in² | -30°C; ISO 179/1eA |
Charpy Impact, Unnotched Low Temp | NB | NB | -30°C; ISO 179/1eU |
Charpy Impact, Notched | 13 J/cm² | 61.9 ft-lb/in² | 23°C, Partial Break; ISO 179/1eA |
Electrical Properties |
|
Volume Resistivity | 1e+012 ohm-cm | 1e+012 ohm-cm | IEC 60093 |
Dielectric Constant | 4.6 | 4.6 | 23°C/1 MHz; IEC 60250 |
Dielectric Constant, Low Frequency | 11 | 11 | 23°C/100 Hz; IEC 60250 |
Dielectric Strength | 30 kV/mm | 762 kV/in | K20/P50; IEC 60243-1 |
Dissipation Factor | 0.19 | 0.19 | 23°C/1 MHz; IEC 60250 |
Dissipation Factor, Low Frequency | 0.2 | 0.2 | 23°C/100 Hz; IEC 60250 |
Comparative Tracking Index | Min 600 V | Min 600 V | Test Solution A, 50 drops; IEC 60112 |
Comparative Tracking Index | 600 V | 600 V | Test Solution A, 100 drops; IEC 60112 |
Thermal Properties |
|
CTE, linear 20°C | 180 µm/m-°C | 100 µin/in-°F | 23-55°C (45x15x10 mm); ISO 11359 |
Melting Point | 172 °C | 342 °F | Peak Temperature; ISO 3146, ISO 11357 |
Deflection Temperature at 0.46 MPa (66 psi) | 100 °C | 212 °F | ISO 75 |
Deflection Temperature at 1.8 MPa (264 psi) | 45 °C | 113 °F | ISO 75 |
Vicat Softening Point | 130 °C | 266 °F | 50N; ISO 306 |
Vicat Softening Point | 165 °C | 329 °F | 10N; ISO 306 |
Flammability, UL94 | HB | HB | 3.2 mm |
Flammability, UL94 | HB | HB | 1.6 mm |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |