Degussa AG Vestamid® X7380 23% Glass, Antistatic, Black, Electrically Conductive Nylon 12
Subcategory: Nylon; Nylon 12; Polymer; Thermoplastic
Key Words: PA12-HI,MHZ,16-050,GF23
Material Notes: Description: Medium-viscosity,23% chopped strands, heat- and light-stabilized, increased impact strength Applications: Quick connectors in conductive fuel lines Information provided by degussa.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.21 g/cc | 0.0437 lb/in³ | ISO 1183 |
| Moisture Absorption at Equilibrium | 0.6 % | 0.6 % | 23°C/50% R.H. (1mm); ISO 62 |
| Water Absorption at Saturation | 1.2 % | 1.2 % | 1 mm; ISO 62 |
| Linear Mold Shrinkage | 0.003 cm/cm | 0.003 in/in | 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2) |
| Linear Mold Shrinkage, Transverse | 0.009 cm/cm | 0.009 in/in | 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2) |
Mechanical Properties |
|
| Tensile Strength at Break | 100 MPa | 14500 psi | ISO 527-1/2 |
| Elongation at Break | 6 % | 6 % | ISO 527-1/2 |
| Tensile Modulus | 5.4 GPa | 783 ksi | ISO 527-1/2 |
| Charpy Impact Unnotched | 8 J/cm² | 38.1 ft-lb/in² | 23°C; ISO 179/1eU |
| Charpy Impact, Notched, Low Temp | 0.8 J/cm² | 3.81 ft-lb/in² | -30°C; ISO 179/1eA |
| Charpy Impact, Unnotched Low Temp | 6 J/cm² | 28.6 ft-lb/in² | -30°C; ISO 179/1eU |
| Charpy Impact, Notched | 1.7 J/cm² | 8.09 ft-lb/in² | 23°C; ISO 179/1eA |
Electrical Properties |
|
| Volume Resistivity | 1e+007 ohm-cm | 1e+007 ohm-cm | IEC 60093 |
| Insulation Resistance | 1e+007 ohm | 1e+007 ohm | Isolation Resistance (ROE DIN 43582:1983/VDE 0303 part 3; IEC 60167 |
Thermal Properties |
|
| CTE, linear 20°C | 40 µm/m-°C | 22.2 µin/in-°F | 23-55°C (45x15x10 mm); ISO 11359 |
| Melting Point | 178 °C | 352 °F | Peak Temperature; ISO 3146, ISO 11357 |
| Deflection Temperature at 0.46 MPa (66 psi) | 175 °C | 347 °F | ISO 75 |
| Deflection Temperature at 1.8 MPa (264 psi) | 160 °C | 320 °F | ISO 75 |
| Vicat Softening Point | 170 °C | 338 °F | 50N; ISO 306 |
| Vicat Softening Point | 175 °C | 347 °F | 10N; ISO 306 |
| Flammability, UL94 | HB | HB | 3.2 mm |
| Flammability, UL94 | HB | HB | 1.6 mm |
|
|
 |
Copyright 1996-2010 by Automation Creations, Inc. The information provided by
MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not
be reproduced either electronically, photographically or substantively without permission from
Automation Creations, Inc. No warranty, neither expressed nor implied, is given
regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of
information from MatWeb.
|
 |