Physical PropertiesMetricEnglishComments
Specific Gravity1.43 g/cc0.0517 lb/in³ ASTM D792
Linear Mold Shrinkage0.003 - 0.005 cm/cm0.003 - 0.005 in/in 3.20 mm; ASTM D955
Linear Mold Shrinkage0.008 - 0.01 cm/cm0.008 - 0.01 in/in 6.40 mm; ASTM D955

Mechanical Properties
Tensile Strength, Yield98.1 MPa14200 psi ASTM D638
Elongation at Break3 %3 % ASTM D638
Flexural Modulus5.98 GPa867 ksi ASTM D790
Flexural Strength148 MPa21500 psi ASTM D790
Izod Impact, Notched0.39 J/cm0.731 ft-lb/in ASTM D256

Electrical Properties
Surface Resistance1e+008 - 1e+012 ohm1e+008 - 1e+012 ohm ASTM D257

Thermal Properties
CTE, linear 20°C80 µm/m-°C44.4 µin/in-°F TMA, -30°C to 30°C
Deflection Temperature at 0.46 MPa (66 psi)199 °C390 °F Unannealed (3.20 mm); ASTM D648

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.