MatWeb, The Online Materials Database

LNP (SABIC Innovative Plastics) ULTEM® SMU5832 Polyetherimide, 30% Carbon\Glass\Mineral Reinforced


Subcategory: Filled/Reinforced Thermoplastic; Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
ESD characteristics for ultra high-heat applications. Will be UC3010.

  • Features: High Heat Resistance
  • Forms: Pellets
  • Processing Method: Injection Molding
Information provided by LNP, a GE Plastics Company.

Physical PropertiesOriginal ValueComments
Specific Gravity1.48 g/cc ASTM D792

Mechanical Properties
Tensile Strength at Break127 MPa Type I, 5 mm/min; ASTM D638
Elongation at Break4 % Type I, 5 mm/min; ASTM D638
Flexural Modulus9.65 GPa (102 mm Span) 3mm/min; ASTM D790
Flexural Yield Strength154 MPa (102 mm Span) 3mm/min; ASTM D790
Izod Impact, Notched0.374 J/cm ASTM D256

Electrical Properties
Surface Resistance100000 ohm ASTM D257
Static DecayMax 0.01 sec 5000V to <50V; FTMS101B

Thermal Properties
Deflection Temperature at 1.8 MPa (264 psi)210 °C Unannealed (6.35 mm); ASTM D648

Processing Properties
Rear Barrel Temperature360 - 421 °C 
Middle Barrel Temperature371 - 421 °C 
Front Barrel Temperature382 - 427 °C 
Nozzle Temperature377 - 421 °C 
Melt Temperature382 - 427 °C 
Mold Temperature135 - 163 °C 
Drying Temperature149 °C 
Dry TimeMax 24 hour 
Moisture Content0.02 % Suggested
Back Pressure0.345 - 0.689 MPa 
Clamp Pressure41 - 69 MPa 
Shot Size40 - 60 % Suggested
Vent Depth0.0025 - 0.0076 cm 
Screw Speed40 - 70 rpm 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.