MatWeb, The Online Materials Database

RTP Company RTP 1403 Polyethersulfone (PES) Glass Fiber


Subcategory: Polyethersulfone; Polymer; Thermoplastic

Physical PropertiesOriginal ValueComments
Specific Gravity1.51 g/cc ASTM D792
Filler Content20 % Primary Additive
Water Absorption0.4 % 24 hrs; 23°C; ASTM D570
Linear Mold Shrinkage0.004 cm/cm 1/8 in (3.2 mm); ASTM D955

Mechanical Properties
Hardness, Rockwell R122 ASTM D785
Tensile Strength @ Break19000 psi ASTM D638
Elongation at Break2.9 % ASTM D638
Tensile Modulus1e+006 psi ASTM D638
Flexural Modulus900000 psi ASTM D638
Flexural Yield Strength28000 psi ASTM D790
Izod Impact, Unnotched11 ft-lb/in 1/8 in (3.2 mm); ASTM D4812
Izod Impact, Notched1.4 ft-lb/in 1/8 in (3.2 mm); ASTM D256

Electrical Properties
Volume ResistivityMin 1e+012 ohm-cm ASTM D257
Dielectric Constant3.9 1 MHz; Dry; ASTM D150
Dielectric Strength375 V/mil S/T; in oil; ASTM D149
Dissipation Factor0.007 1 MHz; Dry; ASTM D150
Arc Resistance70 sec ASTM D495

Thermal Properties
CTE, linear 68°F19 µin/in-°F Flow Direction; ASTM E831
Thermal Conductivity2.1 BTU-in/hr-ft²-°F Through Plane; ASTM E1530
Deflection Temperature at 0.46 MPa (66 psi)430 °F ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)420 °F ASTM D648
Flammability, UL94V-0 1/16 in (1.5 mm)

Processing Properties
Melt Temperature650 - 710 °F 
Mold Temperature275 - 350 °F 
Drying Temperature300 °F 6 hrs
Moisture Content0.04 % 
Dew Point-25 °F 
Injection Pressure10000 - 15000 psi 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.