RTP Company RTP 1481 Polyethersulfone (PES) Carbon Fiber


Subcategory: Polyethersulfone; Polymer; Thermoplastic

Physical PropertiesMetricEnglishComments
Specific Gravity1.39 g/cc0.0502 lb/in³ ASTM D792
Filler Content10 %10 % Primary Additive
Water Absorption0.35 %0.35 % 24 hrs; 23°C; ASTM D570
Linear Mold Shrinkage0.002 cm/cm0.002 in/in 1/8 in (3.2 mm); ASTM D955

Mechanical Properties
Tensile Strength @ Break141 MPa20500 psi ASTM D638
Elongation at Break3 %3 % ASTM D638
Tensile Modulus8.96 GPa1300 ksi ASTM D638
Flexural Modulus8.27 GPa1200 ksi ASTM D638
Flexural Yield Strength207 MPa30000 psi ASTM D790
Izod Impact, Unnotched5.87 J/cm11 ft-lb/in 1/8 in (3.2 mm); ASTM D4812
Izod Impact, Notched0.694 J/cm1.3 ft-lb/in 1/8 in (3.2 mm); ASTM D256

Thermal Properties
Deflection Temperature at 1.8 MPa (264 psi)210 °C410 °F ASTM D648
Flammability, UL94V-0V-0 1/16 in (1.5 mm)

Processing Properties
Melt Temperature343 - 377 °C650 - 710 °F 
Mold Temperature135 - 177 °C275 - 350 °F 
Drying Temperature149 °C300 °F 6 hrs
Moisture Content0.04 %0.04 % 
Dew Point-31.7 °C-25 °F 
Injection Pressure68.9 - 103 MPa10000 - 15000 psi 

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.