Physical PropertiesMetricEnglishComments
Density1.12 g/cc0.0405 lb/in³ 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D792

Mechanical Properties
Hardness, Shore A8686 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D2240
Tensile Strength, Ultimate52 MPa7540 psi 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C; ASTM D412
Tensile Strength, Yield19 MPa2760 psi Tensile stress at 300% elongation; 0.76 mm (0.030 in) extruded sheet; ASTM D-412
Tensile Strength, Yield7.6 MPa1100 psi Tensile stress at 100% elongation.; ASTM D-412
Elongation at Break570 %570 % on 0.030 in extruded sheet; ASTM D-412
Flexural Modulus0.043 GPa6.24 ksi 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D790
Tear Strength66 kN/m377 pli Split tear strength (ASTM D-1938) on 0.76 mm ( 0.030 inch) extruded sheet
Graves Tear Strength88 kN/m502 pli on 0.76 mm ( 0.030 inch) extruded sheet; ASTM D624
Taber Abrasion, mg/1000 Cycles2525 H-18 wheel; ASTM D-1044; 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.
Compression Set25 %25 % 22 hr at 23°C per ASTM D-395; 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.
Compression Set, Elevated Temperature45 %45 % 22 hr @ 70°C; ASTM D-395; 0.080 in molded plaque after curing 20 hrs at 100°C.
Tensile Set32 %32 % at 200% elongation per ASTM D-412 is on 0.030 in extruded sheet.

Thermal Properties
Vicat Softening Point100 °C212 °F 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D1525
Glass Temperature-40 °C-40 °F Pellet sample

 


Copyright 1996-2010 by Automation Creations, Inc.  The information provided by MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from Automation Creations, Inc. No warranty, neither expressed nor implied, is given regarding the accuracy of this information. The user assumes all risk and liability in connection with the use of information from MatWeb.