Advanced Elastomer Systems Santoprene® 191-70PA Thermoplastic Rubber
Subcategory: Elastomer, TPE; Polymer; Thermoplastic
Material Notes: A black thermoplastic elastomer especially formulated to be used in combination with polyamide (PA) for applications where hard/soft combinations are required. Since the product bonds to PA, typical applications are corrugated hose and fittings, soft grip handles and wheels with PA hubs. It can be processed using injection molding or extrusion. Key Features: Excellent processing in injection molding; Smooth surface or 'soft touch'; Good rubbery properties; Excellent adhesion onto PA Additional processing comments: This thermoplastic rubber is a shear-dependent material that can be processed on conventional thermoplastic equipment for injection molding or extrusion. For extrusion, a general purpose screw with a compression ratio of 2.5 to 3.0 is recommended. Material can be recycled. SANTOPRENE rubber is incompatible with acetal and PVC. Values below are for injection molded plaques, side gated, 82.6 mm x 117.5 mm x 3.0 mm. Tensile properties measured across flow. Data provided by Advanced Elastomer Systems.
No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
Physical Properties | Metric | English | Comments |
|
Density | 0.95 g/cc | 0.0343 lb/in³ | TPE-0105 (ASTM D792) |
Mechanical Properties |
|
Hardness, Shore A | 70 | 70 | 5 Second; TPE-0169 (ASTM D 2240) |
Tensile Strength, Ultimate | 3.7 MPa | 537 psi | TPE-0153 (ASTM D 412) |
Elongation at Break | 270 % | 270 % | TPE-0153 (ASTM D 412) |
100% Modulus | 0.0023 GPa | 0.334 ksi | TPE-0153 (ASTM D 412) |
Graves Tear Strength | 22 kN/m | 126 pli | TPE-0056 (ASTM D 624) |
Compression Set | 28 % | 28 % | 23°C, 22 hrs.; TPE-0016 (ASTM D 412) |
Compression Set, Elevated Temperature | 41 % | 41 % | 70°C, 22 hrs.; TPE-0016 (ASTM D 412) |
Compression Set, Elevated Temperature | 46 % | 46 % | 100°C, 22 hrs.; TPE-0016 (ASTM D 412) |
Processing Properties |
|
Processing Temperature | 260 - 280 °C | 500 - 536 °F | Recommended |
Mold Temperature | Min 60 °C | Min 140 °F | 2K molding |
Mold Temperature | Min 90 °C | Min 194 °F | insert molding |
Drying Temperature | 82 °C | 180 °F | Desiccant drying for 3 hours recommended |
Dry Time | 3 hour | 3 hour | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|