Advanced Elastomer Systems Santoprene® 203-40 Thermoplastic Rubber

Return to last searchReturn to last search
Printer friendly version Printer friendly versionAdd to Folder:
Excel Download Download to Excel (requires Excel and Windows)
 Export data to your CAD/FEA program

Subcategory: Elastomer, TPE; Polymer; Thermoplastic

Material Notes:
A colorable thermoplastic general purpose elastomer with good fluid resistance, formulated to replace thermoset elastomers such as EPDM, polychloroprene, and chlorosulfonated polyethylene. It can be processed using injection molding, extrusion, blow molding or other melt processing techniques.

Key Features: Dielectric constant 2.3, dielectric strength at 3.17 mm (125 mil), 19.6 kV/mm (500 v/mil); UL Yellow Card listed, UL 94 HB flame rating; Continuous temperature rating 1000 hrs. @ 135°C (275°F); Excellent flex fatigue resistance; Excellent ozone resistance

Additional processing comments: This thermoplastic rubber is a shear-dependent material that can be processed on conventional thermoplastic equipment for injection molding, extrusion, or blow molding. For extrusion, a general purpose screw with a compression ratio of 2.5 to 3.0 is recommended. Material can be recycled. SANTOPRENE rubber is incompatible with acetal and PVC.

Values below are for injection molded plaques, side gated, 82.6 mm x 117.5 mm x 3.0 mm. Tensile properties measured across flow. Data provided by Advanced Elastomer Systems.

No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.

Physical PropertiesMetricEnglishComments
Density0.94 g/cc0.034 lb/in³ TPE-0105 (ASTM D792)

Mechanical Properties
Hardness, Shore D4040 5 Second; TPE-0169 (ASTM D 2240)
Tensile Strength, Ultimate19 MPa2760 psi TPE-0153 (ASTM D 412)
Elongation at Break600 %600 % TPE-0153 (ASTM D 412)
100% Modulus0.0092 GPa1.33 ksi TPE-0153 (ASTM D 412)
Tear Strength65 kN/m371 pli 65 kN/m at 23°C. Value at 100°C is 36 kN/m. TPE-0056 (ASTM D 624)
Compression Set32 %32 % 23°C, 168 hrs.; TPE-0016 (ASTM D 412)
Compression Set, Elevated Temperature49 %49 % 100°C, 168 hrs.; TPE-0016 (ASTM D 412)
Tensile Set48 %48 % 23°C, 168 hrs.; TPE-0053 (ASTM D 412)

Electrical Properties
Dielectric Constant2.32.3 Frequency not specified
Dielectric Strength19.6 kV/mm498 kV/in at 3.17 mm (0.125 in)

Thermal Properties
Maximum Service Temperature, Air135 °C275 °F Continuous temperature Rating, 1000 hours
Brittleness TemperatureMax -57 °CMax -70.6 °F TPE-0089 (ASTM D 746)
Flammability, UL94HBHB 

Processing Properties
Processing Temperature177 - 232 °C351 - 450 °F 
Drying Temperature82 °C180 °F Desiccant drying for 3 hours recommended
Dry Time3 hour3 hour 
Printer friendly version Printer friendly version


Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistant format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

New MatWeb Services

<meta http-equiv=Content-Type content="text/html; charset=UTF-8">
请读关于材料数据的使用许可协议和我们的隐私权。询问或评论有关 MatWeb? 请与webmaster@matweb.com 联系。我们感谢您对 MatWeb的参与。

本站点由 Automation Creations, Inc. 设计和维护。这个网站的内容, MatWeb 的商标,与 "MatWeb" 由 Automation Creations, Inc.版权1996-2006拥有 。 MatWeb 意欲为个人使用 , 非商业用途。这个站点的内容、结果和技术数据,未经由 Automation Creations, Inc. 允许, 不可以被电子,摄影或实质上地再生产或自动化创作。