Advanced Elastomer Systems Santoprene® 211-45 Thermoplastic Rubber
Subcategory: Elastomer, TPE; Polymer; Thermoplastic
Material Notes: A colorable thermoplastic molding grade elastomer with good fluid resistance, formulated to replace thermoset elastomers such as EPDM, polychloroprene, and chlorosulfonated polyethylene. A high-flow material designed for use in difficult injection molding applications. Key Features: Dielectric constant 2.3, dielectric strength at 3.17 mm (125 mil), 19.6 kV/mm (500 v/mil); Excellent flex fatigue resistance; Excellent ozone resistance; Flex modulus at Tangent 5.5 MPa (800 psi); Excellent sealing properties Additional processing comments: This thermoplastic rubber is a shear-dependent material that can be processed on conventional thermoplastic equipment for injection molding, extrusion, or blow molding. For extrusion, a general purpose screw with a compression ratio of 2.5 to 3.0 is recommended. Material can be recycled. SANTOPRENE rubber is incompatible with acetal and PVC. Values below are for injection molded plaques, side gated, 82.6 mm x 117.5 mm x 3.0 mm. Tensile properties measured across flow. Data provided by Advanced Elastomer Systems.
No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
Physical Properties | Metric | English | Comments |
|
Density | 0.96 g/cc | 0.0347 lb/in³ | TPE-0105 (ASTM D792) |
Mechanical Properties |
|
Hardness, Shore A | 45 | 45 | 5 Second; TPE-0169 (ASTM D 2240) |
Tensile Strength, Ultimate | 3.8 MPa | 551 psi | TPE-0153 (ASTM D 412) |
Elongation at Break | 330 % | 330 % | TPE-0153 (ASTM D 412) |
100% Modulus | 0.0015 GPa | 0.218 ksi | TPE-0153 (ASTM D 412) |
Flexural Modulus | 0.0055 GPa | 0.798 ksi | Tangent |
Tear Strength | 13.7 kN/m | 78.2 pli | at 23°C. Value at 100°C is 4.9 kN/m. TPE-0056 (ASTM D 624) |
Compression Set | 13 % | 13 % | 23°C, 22 hrs.; TPE-0016 (ASTM D 412) |
Compression Set, Elevated Temperature | 22 % | 22 % | 100°C, 22 hrs.; TPE-0016 (ASTM D 412) |
Tensile Set | 5 % | 5 % | 23°C, 22 hrs.; per TPE-0053 (ASTM D 412) |
Electrical Properties |
|
Dielectric Constant | 2.3 | 2.3 | Frequency not specified |
Dielectric Strength | 19.6 kV/mm | 498 kV/in | at 3.17 mm (0.125 in) |
Thermal Properties |
|
Brittleness Temperature | Max -60 °C | Max -76 °F | TPE-0089 (ASTM D 746) |
Processing Properties |
|
Processing Temperature | 177 - 232 °C | 351 - 450 °F | |
Drying Temperature | 82 °C | 180 °F | Desiccant drying for 3 hours recommended |
Dry Time | 3 hour | 3 hour | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|