BASF Petra 110 BK-112 PET, 15% Glass Filled
Subcategory: Polyester, TP; Polyethylene Terephthalate (PET); Polymer; Thermoplastic
Material Notes: Information provided by BASF Corporation.
No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.44 g/cc | 0.052 lb/in³ | ISO 1183 |
| Linear Mold Shrinkage | 0.005 cm/cm | 0.005 in/in | MD; ASTM Test |
Mechanical Properties |
|
| Tensile Strength, Ultimate | 105 MPa | 15200 psi | 5 mm/min; ISO 527 |
| Tensile Strength at Break | 105 MPa | 15200 psi | 0.2 in/min; ASTM D638 |
| Elongation at Break | 3.5 % | 3.5 % | 5 mm/min; ISO 527 |
| Elongation at Break | 3.5 % | 3.5 % | 0.2 in/min; ASTM D638 |
| Tensile Modulus | 6.68 GPa | 969 ksi | 1 mm/min; ISO 527 |
| Flexural Modulus | 5.35 GPa | 776 ksi | ASTM D790 |
| Flexural Modulus | 5.48 GPa | 795 ksi | ISO 178 |
| Flexural Strength | 145 MPa | 21000 psi | ASTM D790 |
| Izod Impact, Notched (ISO) | 6 kJ/m² | 2.86 ft-lb/in² | ISO 180 |
| Charpy Impact, Notched | 0.6 J/cm² | 2.86 ft-lb/in² | ISO 179 |
| Izod Impact, Notched | 0.0065 J/cm | 0.0122 ft-lb/in | ASTM D256 |
Electrical Properties |
|
| Dielectric Constant | 3.3 | 3.3 | 1 MHz; IEC 60250 |
| Dielectric Constant | 3.4 | 3.4 | 100 Hz; IEC 60250 |
| Dielectric Strength | 36 kV/mm | 914 kV/in | IEC 60243-1 |
| Dissipation Factor | 0.01 | 0.01 | 100 Hz; IEC 60250 |
| Dissipation Factor | 0.02 | 0.02 | 1 MHz; IEC 60250 |
Thermal Properties |
|
| CTE, linear 20°C | 32 µm/m-°C | 17.8 µin/in-°F | Parallel; ISO 11359 |
| CTE, linear 20°C Transverse to Flow | 79 µm/m-°C | 43.9 µin/in-°F | ISO 11359 |
| Melting Point | 245 °C | 473 °F | 10 K/min |
| Melting Point | 245 °C | 473 °F | ASTM D3418 |
| Deflection Temperature at 0.46 MPa (66 psi) | 231 °C | 448 °F | ISO 75 |
| Deflection Temperature at 1.8 MPa (264 psi) | 192 °C | 378 °F | ISO 75 |
| Deflection Temperature at 1.8 MPa (264 psi) | 208 °C | 406 °F | ASTM D648 |
| Flammability, UL94 | HB | HB | 0.81 mm |
| Flammability, UL94 | HB | HB | 3 mm |
Processing Properties |
|
| Melt Temperature | 275 °C | 527 °F | Injection molding |
| Mold Temperature | 115 °C | 239 °F | Injection molding |
Descriptive Properties | |
| Additive | Fillers | |
| Color | BK-112 | |
| Commercial Status (March 2007) | Active America | |
| Form | Pellets | |
| Impact Modified | No | |
| Injection molding | Processable | |
| Primary Processing Technique | Injection Molding | |
| UL.UL-C | Yes | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.

|