Arkema Rilsan® AZM 15 TLD Nylon 12, 15% Glass Fiber Filled (Conditioned)
Subcategory: Filled/Reinforced Thermoplastic; Nylon; Nylon 12; Polymer; Thermoplastic
Close Analogs: Arkema, formed in 2004, was formerly Atofina Chemicals and before that Elf Atochem.
Key Words: PA12; Polyamide 12
Material Notes: Designation ISO 1874-PA12,MHLR,16-030,GF15 Rigid grade with glass fiber filler (15%) for injection molding. Available color: natural. Light and heat stabilized. Mold-release agent. Rigidity combined with good impact strength. High compressive strength. Very low shrinkage: include 0,5% on average for the design of the mold. Low coefficient of linear expansion. High dimensional stability. Example applications: Mechanical fittings. ISO data provided by the manufacturer, Arkema.
No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
Physical Properties | Metric | English | Comments |
|
Melt Flow | 12.9 g/10 min | 12.9 g/10 min | 235°C/2.16 kg load |
Mechanical Properties |
|
Tensile Strength, Ultimate | 72 MPa | 10400 psi | 5 mm/min |
Elongation at Break | 8 % | 8 % | 5 mm/min |
Tensile Modulus | 3.83 GPa | 556 ksi | 1 mm/min |
Charpy Impact Unnotched | 6.4 J/cm² | 30.5 ft-lb/in² | |
Charpy Impact, Notched, Low Temp | 0.72 J/cm² | 3.43 ft-lb/in² | at -30°C |
Charpy Impact, Unnotched Low Temp | 6.87 J/cm² | 32.7 ft-lb/in² | at -30°C |
Charpy Impact, Notched | 1.15 J/cm² | 5.47 ft-lb/in² | |
Thermal Properties |
|
Vicat Softening Point | 151 °C | 304 °F | 50°C/hr; 50N |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|