Physical Properties | Metric | English | Comments |
|
Density | 1.14 g/cc | 0.0412 lb/in³ | ASTM D 792 |
Linear Mold Shrinkage | 0.005 - 0.007 cm/cm | 0.005 - 0.007 in/in | Flow, 0.125 inch; ASTM D 955 |
Melt Flow | 12 g/10 min | 12 g/10 min | 260C/3.8 kgf; ASTM D 1238 |
Mechanical Properties |
|
Tensile Strength @ Yield | 59.3 MPa | 8600 psi | Type I, 2.0 in/min; ASTM D 638 |
Elongation at Break | 75 % | 75 % | Type I, 2.0 in/min; ASTM D 638 |
Elongation at Yield | 5 % | 5 % | Type I, 2.0 in/min; ASTM D 638 |
Tensile Modulus | 2.21 GPa | 320 ksi | 2.0 in/min; ASTM D 638 |
Flexural Modulus | 2.38 GPa | 345 ksi | 0.05 in/min, 2" span; ASTM D 790 |
Flexural Yield Strength | 86.9 MPa | 12600 psi | 0.05 in/min, 2" span; ASTM D 790 |
Izod Impact, Notched, Low Temp | 2.67 J/cm | 5 ft-lb/in | at -22F; ASTM D 256 |
Gardner Impact @ 23°C | 47.5 J | 35 ft-lb | Instrumented Impact Energy @ peak, -22°F; ASTM D 3763 |
Gardner Impact @ 23°C | 54.2 J | 40 ft-lb | Instrumented Impact Energy @ peak, -22°F; ASTM D 3763 |
Gardner Impact @ 23°C | 61 J | 45 ft-lb | Instrumented Impact Energy @ peak, 73F; ASTM D 3763 |
Gardner Impact @ 23°C | 61 J | 45 ft-lb | Instrumented Impact Total Energy, 73°F; ASTM D 3763 |
Izod Impact, Notched | 6.41 J/cm | 12 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
Arc Resistance | 120 - 180 sec | 120 - 180 sec | Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495 |
Comparative Tracking Index | 175 - 250 V | 175 - 250 V | (+/- 0.125 inch); PLC Code 3; UL 746A |
Hot Wire Ignition, HWI | 15 - 30 sec | 15 - 30 sec | (+/- 0.125 inch); PLC Code 3; UL 746A |
High Amp Arc Ignition, HAI | Min 120 arcs | Min 120 arcs | Surface (+/- 0.125 inch); PLC Code 0; UL 746A |
High Voltage Arc-Tracking Rate, HVTR | 10 - 25.4 mm/min | 0.394 - 1 in/min | (+/- 0.125 inch); PLC Code 1; UL 746A |
Thermal Properties |
|
CTE, linear 68°F | 72 µm/m-°C | 40 µin/in-°F | Flow, -22F to 86F; ASTM D 696 |
Deflection Temperature at 0.46 MPa (66 psi) | 127 °C | 260 °F | 0.125 inch, unannealed; ASTM D 648 |
Deflection Temperature at 1.8 MPa (264 psi) | 110 °C | 230 °F | 0.125 inch, unannealed; ASTM D 648 |
UL RTI, Electrical | 60 °C | 140 °F | UL 746B |
UL RTI, Mechanical with Impact | 60 °C | 140 °F | UL 746B |
UL RTI, Mechanical without Impact | 60 °C | 140 °F | UL 746B |
Flammability, UL94 | HB | HB | 0.048 in. |
Descriptive Properties |
|
CSA File No. | LS88480 | |
UL File Number, USA | E121562 | |
UV-light, water exposure/immersion | F2 | UL746C |
|