SABIC Innovative Plastics CYCOLOY C6200 ABS + Polycarbonate (North America)
Subcategory: ABS Polymer; Polycarbonate; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.18 g/cc | 0.0426 lb/in³ | ASTM D 792 |
| Linear Mold Shrinkage | 0.004 - 0.006 cm/cm | 0.004 - 0.006 in/in | Flow, 0.125 inch; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.004 - 0.006 cm/cm | 0.004 - 0.006 in/in | 0.125 inch; ASTM D 955 |
| Melt Flow | 14.5 g/10 min | 14.5 g/10 min | 260C/2.16 kgf; ASTM D 1238 |
| Spiral Flow | 68.6 cm | 27 in | 500F, 10 ips, .125 X 60 in |
Mechanical Properties |
|
| Tensile Strength @ Yield | 66.9 MPa | 9700 psi | Type I, 2.0 in/min; ASTM D 638 |
| Elongation at Break | 50 % | 50 % | Type I, 2.0 in/min; ASTM D 638 |
| Flexural Modulus | 2.69 GPa | 390 ksi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Yield Strength | 103 MPa | 15000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Gardner Impact @ 23°C | 54.2 J | 40 ft-lb | Instrumented Impact Energy @ peak, -22°F; ASTM D 3763 |
| Gardner Impact @ 23°C | 61 J | 45 ft-lb | Instrumented Impact Energy @ peak, 73F; ASTM D 3763 |
| Izod Impact, Notched | 5.34 J/cm | 10 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Volume Resistivity | Min 1e+015 ohm-cm | Min 1e+015 ohm-cm | IEC 60093 |
| Surface Resistivity per Square | Min 1e+015 ohm | Min 1e+015 ohm | IEC 60093 |
| Dielectric Constant | 2.7 | 2.7 | 1 MHz; IEC 60250 |
| Dielectric Constant | 2.8 | 2.8 | 50 Hz; IEC 60250 |
| Dielectric Strength | 17 kV/mm | 432 kV/in | in oil, 3.2 mm; IEC 60243-1 |
| Dielectric Strength | 25 kV/mm | 635 kV/in | in oil, 1.6 mm; IEC 60243-1 |
| Dielectric Strength | 35 kV/mm | 889 kV/in | in oil, 0.8 mm; IEC 60243-1 |
| Dissipation Factor | 0.004 | 0.004 | 50 Hz; IEC 60250 |
| Dissipation Factor | 0.008 | 0.008 | 1 MHz; IEC 60250 |
| Arc Resistance | 60 - 120 sec | 60 - 120 sec | Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495 |
| Comparative Tracking Index | 250 - 400 V | 250 - 400 V | (+/- 0.125 inch); PLC Code 2; UL 746A |
| Hot Wire Ignition, HWI | 30 - 60 sec | 30 - 60 sec | (+/- 0.125 inch); PLC Code 2; UL 746A |
| High Amp Arc Ignition, HAI | Min 120 arcs | Min 120 arcs | Surface (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | 80 - 150 mm/min | 3.15 - 5.91 in/min | (+/- 0.125 inch); PLC Code 3; UL 746A |
Thermal Properties |
|
| Deflection Temperature at 1.8 MPa (264 psi) | 87.8 °C | 190 °F | 0.125 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 90.6 °C | 195 °F | 0.250 inch, unannealed; ASTM D 648 |
| UL RTI, Electrical | 85 °C | 185 °F | UL 746B |
| UL RTI, Mechanical with Impact | 85 °C | 185 °F | UL 746B |
| UL RTI, Mechanical without Impact | 85 °C | 185 °F | UL 746B |
| Flammability, UL94 | HB | HB | 0.028 in. |
| Flammability, UL94 | V-1 | V-1 | 0.048 in. |
| Flammability, UL94 | V-0 | V-0 | 0.058 in. |
| Flammability, UL94 | 6 | 6 | 0.079 in. |
| Flammability, UL94 | 7 | 7 | 0.134 in. |
Descriptive Properties | |
| CSA File No. | LS88480 | |
| UL File Number, GLOBAL | E161759 | |
| UL File Number, USA | E121562 | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|