| Physical Properties | Metric | English | Comments | 
 | 
| Density | 1.13 g/cc | 0.0408 lb/in³ |  ASTM D 792 | 
| Water Absorption | 0.1 % | 0.1 % |  24 hours @ 73F; ASTM D 570 | 
| Water Absorption at Saturation | 0.4 % | 0.4 % |  Equilibrium, 73F; ASTM D 570 | 
| Linear Mold Shrinkage | 0.005 - 0.007 cm/cm | 0.005 - 0.007 in/in |  Flow, 0.125 inch; ASTM D 955 | 
| Linear Mold Shrinkage, Transverse | 0.005 - 0.007 cm/cm | 0.005 - 0.007 in/in |  0.125 inch; ASTM D 955 | 
| Melt Flow | 17 g/10 min | 17 g/10 min |  260C/5.0 kgf; ASTM D 1238 | 
 Mechanical Properties | 
 | 
| Hardness, Rockwell R | 118 | 118 |  ASTM D 785 | 
| Tensile Strength @ Yield | 54.5 MPa | 7900 psi |  Type I, 2.0 in/min; ASTM D 638 | 
| Elongation at Break | 75 % | 75 % |  Type I, 2.0 in/min; ASTM D 638 | 
| Flexural Modulus | 2.31 GPa | 335 ksi |  0.05 in/min, 2" span; ASTM D 790 | 
| Flexural Yield Strength | 84.8 MPa | 12300 psi |  0.05 in/min, 2" span; ASTM D 790 | 
| Izod Impact, Notched, Low Temp | 3.2 J/cm | 6 ft-lb/in |  at -22F; ASTM D 256 | 
| Gardner Impact @ 23°C | 33.9 J | 25 ft-lb |  Instrumented Impact Total Energy, -22F; ASTM D 3763 | 
| Gardner Impact @ 23°C | 40.7 J | 30 ft-lb |  Instrumented Impact Total Energy, 73°F; ASTM D 3763 | 
| Izod Impact, Notched | 5.34 J/cm | 10 ft-lb/in |  73F; ASTM D 256 | 
 Electrical Properties | 
 | 
| Arc Resistance | 60 - 120 sec | 60 - 120 sec |  Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495 | 
| Comparative Tracking Index | 250 - 400 V | 250 - 400 V |  (+/- 0.125 inch); PLC Code 2; UL 746A | 
| Hot Wire Ignition, HWI | 30 - 60 sec | 30 - 60 sec |  (+/- 0.125 inch); PLC Code 2; UL 746A | 
| High Amp Arc Ignition, HAI | Min 120 arcs | Min 120 arcs |  Surface (+/- 0.125 inch); PLC Code 0; UL 746A | 
 Thermal Properties | 
 | 
| CTE, linear, 212°F (100°C) | 72 µm/m-°C | 40 µin/in-°F |  Flow, 0F to 300F; ASTM E 831 | 
| CTE, linear, 212°F (100°C) | 72 µm/m-°C | 40 µin/in-°F |  Cross Flow; 0F to 300F; ASTM E 831 | 
| Thermal Conductivity | 0.2 W/m-K | 1.39 BTU-in/hr-ft²-°F |  ASTM C 177 | 
| Deflection Temperature at 0.46 MPa (66 psi) | 124 °C | 255 °F |  0.125 inch, unannealed; ASTM D 648 | 
| Deflection Temperature at 0.46 MPa (66 psi) | 129 °C | 265 °F |  0.250 inch, unannealed; ASTM D 648 | 
| Deflection Temperature at 1.8 MPa (264 psi) | 107 °C | 225 °F |  0.125 inch, unannealed; ASTM D 648 | 
| Deflection Temperature at 1.8 MPa (264 psi) | 110 °C | 230 °F |  0.250 inch, unannealed; ASTM D 648 | 
| Vicat Softening Point | 129 °C | 265 °F |  Rate B; ASTM D 1525 | 
| UL RTI, Electrical | 60 °C | 140 °F |  UL 746B | 
| UL RTI, Mechanical with Impact | 60 °C | 140 °F |  UL 746B | 
| UL RTI, Mechanical without Impact | 60 °C | 140 °F |  UL 746B | 
| Flammability, UL94 | HB | HB |  0.059 in. | 
 Optical Properties | 
 | 
| Gloss | 30 % | 30 % |  Untextured, 60 degrees; ASTM D 523 | 
 Descriptive Properties | 
 | 
| CSA File No. | LS88480 |   | 
| UL File Number, USA | E121562 |   | 
 | 
  Printer friendly version |