COMSOL CD

SABIC Innovative Plastics ULTEM 1000M Polyetherimide (North America)

Return to last searchReturn to last search
Printer friendly version Printer friendly versionAdd to Folder:
Excel Download Download to Excel (requires Excel and Windows)
 Export data to your CAD/FEA program

Subcategory: Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line.

Physical PropertiesMetricEnglishComments
Density1.27 g/cc0.0459 lb/in³ ASTM D 792
Water Absorption0.25 %0.25 % 24 hours @ 73F; ASTM D 570
Water Absorption at Saturation1.25 %1.25 % Equilibrium, 73F; ASTM D 570
Linear Mold Shrinkage0.005 - 0.007 cm/cm0.005 - 0.007 in/in Flow, 0.125 inch; ASTM D 955
Melt Flow9.7 g/10 min9.7 g/10 min 337C/6.6 kgf; ASTM D 1238

Mechanical Properties
Hardness, Rockwell M109109 ASTM D 785
Tensile Strength @ Yield110 MPa16000 psi Type I, 0.2 in/min; ASTM D 638
Elongation at Break60 %60 % Type I, 0.2 in/min; ASTM D 638
Elongation at Yield7 %7 % Type I, 0.2 in/min; ASTM D 638
Tensile Modulus3.59 GPa520 ksi 0.2 in/min; ASTM D 638
Flexural Modulus3.52 GPa510 ksi 0.10 in/min, 4" span; ASTM D 790
Flexural Yield Strength165 MPa24000 psi 0.10 in/min, 4" span; ASTM D 790
Poisson's Ratio0.360.36 ASTM D 638
Izod Impact, Unnotched13.3 J/cm25 ft-lb/in 73F; ASTM D 4812
Gardner Impact36.6 J27 ft-lb 73F; ASTM D 3029
Taber Abrasion, mg/1000 Cycles1010 CS-17, 1 kg; ASTM D 1044
Izod Impact, Notched0.534 J/cm1 ft-lb/in 73F; ASTM D 256
Izod Impact, Notched16 J/cm30 ft-lb/in Reverse Notched, 73F; ASTM D 256

Electrical Properties
Volume Resistivity1e+017 ohm-cm1e+017 ohm-cm ASTM D 257
Dielectric Constant3.153.15 1 kHz; ASTM D 150
Dielectric Strength28 kV/mm710 V/mil in oil, 62 mils; ASTM D 149
Dielectric Strength32.7 kV/mm831 V/mil in air, 62 mils; ASTM D 149
Dissipation Factor0.00130.0013 1 kHz; ASTM D 150
Dissipation Factor0.00250.0025 2450 MHz; ASTM D 150

Thermal Properties
CTE, linear, 212°F (100°C)54 µm/m-°C30 µin/in-°F Cross Flow; 0F to 300F; ASTM E 831
CTE, linear, 212°F (100°C)55.8 µm/m-°C31 µin/in-°F Flow, 0F to 300F; ASTM E 831
Thermal Conductivity0.22 W/m-K1.53 BTU-in/hr-ft²-°F ASTM C 177
Deflection Temperature at 0.46 MPa (66 psi)210 °C410 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)201 °C394 °F 0.250 inch, unannealed; ASTM D 648
Vicat Softening Point219 °C426 °F Rate B; ASTM D 1525
Flammability, UL94V-0V-0 0.016 in.
NBS Smoke Density0.70.7 Flaming, Ds 4 min; ASTM E 662
NBS Smoke Density3030 Flaming, Dmax 20 min; ASTM E 662
Oxygen Index47 %47 % ASTM D 2863
Printer friendly version Printer friendly version


Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistant format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Instant Quotes for Quick Parts!Upload your 3D CAD model, select process, quantity, material, and instantly receive your unique, binding quote.

<meta http-equiv=Content-Type content="text/html; charset=UTF-8">
请读关于材料数据的使用许可协议和我们的隐私权。询问或评论有关 MatWeb? 请与webmaster@matweb.com 联系。我们感谢您对 MatWeb的参与。

本站点由 Automation Creations, Inc. 设计和维护。这个网站的内容, MatWeb 的商标,与 "MatWeb" 由 Automation Creations, Inc.版权1996-2006拥有 。 MatWeb 意欲为个人使用 , 非商业用途。这个站点的内容、结果和技术数据,未经由 Automation Creations, Inc. 允许, 不可以被电子,摄影或实质上地再生产或自动化创作。