SABIC Innovative Plastics ULTEM 1010R Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.27 g/cc | 0.0459 lb/in³ | ASTM D 792 |
| Water Absorption | 0.25 % | 0.25 % | 24 hours @ 73F; ASTM D 570 |
| Water Absorption at Saturation | 1.25 % | 1.25 % | Equilibrium, 73F; ASTM D 570 |
| Linear Mold Shrinkage | 0.005 - 0.007 cm/cm | 0.005 - 0.007 in/in | Flow, 0.125 inch; ASTM D 955 |
| Melt Flow | 17.8 g/10 min | 17.8 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Hardness, Rockwell M | 109 | 109 | ASTM D 785 |
| Tensile Strength @ Yield | 110 MPa | 16000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 60 % | 60 % | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Yield | 7 % | 7 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 3.59 GPa | 520 ksi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 3.52 GPa | 510 ksi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Yield Strength | 165 MPa | 24000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Izod Impact, Unnotched | 13.3 J/cm | 25 ft-lb/in | 73F; ASTM D 4812 |
| Gardner Impact | 33.9 J | 25 ft-lb | 73F; ASTM D 3029 |
| Taber Abrasion, mg/1000 Cycles | 10 | 10 | CS-17, 1 kg; ASTM D 1044 |
| Izod Impact, Notched | 0.32 J/cm | 0.6 ft-lb/in | 73F; ASTM D 256 |
| Izod Impact, Notched | 14.9 J/cm | 28 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Electrical Properties |
|
| Volume Resistivity | 1e+017 ohm-cm | 1e+017 ohm-cm | ASTM D 257 |
| Dielectric Constant | 3.15 | 3.15 | 1 kHz; ASTM D 150 |
| Dielectric Strength | 28 kV/mm | 710 V/mil | in oil, 62 mils; ASTM D 149 |
| Dielectric Strength | 32.7 kV/mm | 830 V/mil | in air, 62 mils; ASTM D 149 |
| Dissipation Factor | 0.0013 | 0.0013 | 1 kHz; ASTM D 150 |
| Dissipation Factor | 0.0025 | 0.0025 | 2450 MHz; ASTM D 150 |
| Arc Resistance | 120 - 180 sec | 120 - 180 sec | Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495 |
| Comparative Tracking Index | 100 - 175 V | 100 - 175 V | (+/- 0.125 inch); PLC Code 4; UL 746A |
| Hot Wire Ignition, HWI | 60 - 120 sec | 60 - 120 sec | (+/- 0.125 inch); PLC Code 1; UL 746A |
| High Amp Arc Ignition, HAI | 15 - 30 arcs | 15 - 30 arcs | Surface (+/- 0.125 inch); PLC Code 3; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | 25.4 - 80 mm/min | 1 - 3.15 in/min | (+/- 0.125 inch); PLC Code 2; UL 746A |
Thermal Properties |
|
| CTE, linear, 212°F (100°C) | 55.8 µm/m-°C | 31 µin/in-°F | Flow, 0F to 300F; ASTM E 831 |
| Thermal Conductivity | 0.22 W/m-K | 1.53 BTU-in/hr-ft²-°F | ASTM C 177 |
| Deflection Temperature at 0.46 MPa (66 psi) | 207 °C | 405 °F | 0.250 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 199 °C | 390 °F | 0.250 inch, unannealed; ASTM D 648 |
| Vicat Softening Point | 219 °C | 426 °F | Rate B; ASTM D 1525 |
| UL RTI, Electrical | 170 °C | 338 °F | UL 746B |
| UL RTI, Mechanical with Impact | 170 °C | 338 °F | UL 746B |
| UL RTI, Mechanical without Impact | 170 °C | 338 °F | UL 746B |
| Flammability, UL94 | V-2 | V-2 | 0.028 in. |
| Flammability, UL94 | V-0 | V-0 | 0.028 in. |
| Flammability, UL94 | 7 | 7 | 0.118 in. |
| NBS Smoke Density | 2 | 2 | Flaming, Ds 4 min; ASTM E 662 |
| NBS Smoke Density | 39 | 39 | Flaming, Dmax 20 min; ASTM E 662 |
| Oxygen Index | 44 % | 44 % | ASTM D 2863 |
Descriptive Properties | |
| UL File Number, USA | E121562 | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|