| Physical Properties | Metric | English | Comments |
|
| Density | 1.35 g/cc | 0.0488 lb/in³ | ASTM D 792 |
| Linear Mold Shrinkage | 0.007 - 0.009 cm/cm | 0.007 - 0.009 in/in | Flow, 0.125 inch; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.006 - 0.008 cm/cm | 0.006 - 0.008 in/in | 0.125 inch; ASTM D 955 |
| Melt Flow | 19 g/10 min | 19 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Break | 119 MPa | 17300 psi | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 119 MPa | 17300 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 3 % | 3 % | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Yield | 3 % | 3 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 5.24 GPa | 760 ksi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 0.49 GPa | 71 ksi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Modulus | 5.17 GPa | 750 ksi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Strength | 193 MPa | 28000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Yield Strength | 200 MPa | 29000 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Izod Impact, Unnotched | 5.34 J/cm | 10 ft-lb/in | 73F; ASTM D 4812 |
| Gardner Impact @ 23°C | 10.8 J | 8 ft-lb | Instrumented Impact Total Energy, 73°F; ASTM D 3763 |
| Izod Impact, Notched | 0.694 J/cm | 1.3 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Arc Resistance | 60 - 120 sec | 60 - 120 sec | Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495 |
| Comparative Tracking Index | 100 - 175 V | 100 - 175 V | (+/- 0.125 inch); PLC Code 4; UL 746A |
| Hot Wire Ignition, HWI | 60 - 120 sec | 60 - 120 sec | (+/- 0.125 inch); PLC Code 1; UL 746A |
| High Amp Arc Ignition, HAI | 15 - 30 arcs | 15 - 30 arcs | Surface (+/- 0.125 inch); PLC Code 3; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | 80 - 150 mm/min | 3.15 - 5.91 in/min | (+/- 0.125 inch); PLC Code 3; UL 746A |
Thermal Properties |
|
| CTE, linear 68°F | 36 µm/m-°C | 20 µin/in-°F | Flow, -40F to 100F; ASTM E 831 |
| CTE, linear 68°F, Transverse to Flow | 81 µm/m-°C | 45 µin/in-°F | from -40F to 100F; ASTM E 831 |
| Deflection Temperature at 0.46 MPa (66 psi) | 210 °C | 410 °F | 0.125 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 0.46 MPa (66 psi) | 213 °C | 415 °F | 0.250 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 205 °C | 401 °F | 0.125 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 207 °C | 405 °F | 0.250 inch, unannealed; ASTM D 648 |
| Vicat Softening Point | 210 °C | 410 °F | Rate B; ASTM D 1525 |
| UL RTI, Electrical | 105 °C | 221 °F | UL 746B |
| UL RTI, Mechanical with Impact | 105 °C | 221 °F | UL 746B |
| UL RTI, Mechanical without Impact | 105 °C | 221 °F | UL 746B |
| Flammability, UL94 | V-0 | V-0 | 0.016 in. |
Descriptive Properties |
|
| UL File Number, USA | E121562 | |
|